Key takeaways
- Visual inspection of liquid-applied waterproofing is misleading: only the quantity applied guarantees the required thickness.
- Standard SIA 248 requires continuous waterproofing whose performance depends on compliance with manufacturers' consumption rates.
- Systematic application in two cross coats prevents localized gaps and ensures a homogeneous film thickness.
- Methodical weighing of buckets before and after application provides indisputable arithmetic proof on the construction site.
Calculate the theoretical mass and weigh the containers on the construction site
On construction sites in Romandie, the most frequent error consists in judging a liquid resin or flexible waterproofing mortar by its opacity. A pigmented film perfectly masks the mineral substrate starting from three hundred micrometres, whereas technical data sheets commonly require one millimetre of dry film to guarantee water impermeability under moderate pressure. The tile-laying craftsman cannot rely on the colour: the final thickness depends exclusively on the quantity of material applied per unit area. The calculation must be established before opening the first bucket, integrating the total floor area and vertical perimeter flashings.
- Precise measurement of the waterproofed areaCalculate the area of the shower or bathroom floor, then add the area of the waterproofing flashings against the partitions (at least fifteen centimetres above the finished floor or two metres in the area of water spray zones).
- Determination of the required net weightMultiply this developed area by the consumption per square metre prescribed in the technical data sheet to obtain the regulatory dry film.
- Control weighing before and after coatWeigh the containers on a site spring balance or a calibrated electronic scale. Note the initial mass of the opened bucket, apply the first coat, then weigh the remainder to verify that exactly half of the calculated product has been applied.
- Recording in the site reportRecord the number of containers consumed, the production batch and the treated area on the self-inspection sheet to provide indisputable traceability to the site management.
If the theoretical calculation indicates that a ten-square-metre room requires twenty kilograms of product to reach the required dry thickness and a quarter of the twenty-five-kilogram bucket remains after application, the prescribed thickness has not been reached. This mathematical finding prevents any subsequent dispute: the tiler immediately knows that an additional build coat is essential before starting the tile installation.
Cross two successive coats and measure the thickness of the fresh film
Obtaining a continuous and watertight membrane under tiles relies on a strict execution rule: application in two distinct, cross coats. The first coat's mission is to saturate the substrate roughness and fill residual micro-porosities after the application of the primer. It is generally applied with a wide brush or a medium-pile roller in a constant linear direction, for example vertically on walls and lengthwise on the floor. This initial pass also serves to embed corner reinforcement tapes and pipe sleeves without forming creases.
Waterproofing under tiles must form a continuous, adherent and regularly thick barrier, capable of bridging substrate micro-cracks without presenting localized weaknesses.
norme SIA 248
| Execution phase | Recommended tool | Target thickness (fresh) | Application direction |
|---|---|---|---|
| First coat | Roller or smooth trowel | Half of the total thickness | Longitudinal / vertical direction |
| Drying interval | Touch check | Film set throughout | Not passable by foot traffic |
| Second coat | Roller or smooth trowel | Compliant final thickness | Crossed perpendicularly |
| Spot check | Wet film gauge (comb) | Technical data sheet value | Measurement at strategic points |
The second coat can only begin when the first is sufficiently dry so as not to be torn or soaked by the passage of the tool, while retaining a surface reactivity conducive to chemical cohesion between the two coats. This second application must be carried out at a right angle to the previous one. This methodical crossing makes it possible to fill any material shortages, micro-bubbles or grooves left by the roller during the first coat. Some manufacturers offer contrasting colours for each coat, which greatly facilitates the visual identification of under-dosed areas during the application of the second coat.
In addition to weighing the containers, the team leader carries out instantaneous measurements on the still fresh product using a wet film thickness gauge. This notched stainless steel instrument is placed perpendicularly to the freshly coated substrate on several critical areas, in particular at the junction of flashings and around floor drains. Reading the highest tooth wetted by the paste gives the immediate wet thickness. By knowing the dry extract of the product indicated on the technical data sheet, this reading confirms on the spot that the final dry film will reach the value required by standard SIA 248.
Material balance by container weighing and surface validation
Visual examination of a liquid membrane after drying is misleading: a homogeneous shade and a continuous film in no way attest to the presence of the prescribed protective millimetre. An experienced applicator knows that a pass pulled out excessively with a roller can give a false impression of uniformity while showing a thickness deficit of half. The only objective means of guaranteeing the conformity of the work without altering the membrane consists in comparing the actual treated area with the exact mass of spread product. According to standard SIA 248, the application of liquid-applied waterproofing systems requires metrological rigour throughout operations, from substrate acceptance to the installation of ceramic tiling.
- Contradictory measurement of the treated areaRecord the actual dimensions of the walls and floor waterproofed, including vertical returns of at least fifteen centimetres and shower tray drops. For a standard cabin of 0.90 m by 0.90 m with a protected height of 2.00 m, the developed area reaches approximately 7.60 m² excluding the floor.
- Differential weighing of containersPlace each opened bucket on a spring balance or site scale before and after application. The initial gross mass minus the residual mass and the tare of the empty packaging provides the exact weight of paste applied on the construction site.
- Calculation of the effective consumption ratioDivide the net mass applied by the measured measurement. If the calculation shows a consumption of 0.85 kg/m² whereas the technical data sheet of the system requires 1.2 kg/m² to reach the dry thickness required by standard SIA 248, the membrane is structurally non-compliant, regardless of the regularity of its surface appearance.
- Recording in the site reportRecord on the daily report the covered area, the batch numbers of the buckets used, the net masses consumed and the theoretical dry thickness calculated according to the dry extract of the product.
| Deviation noted during weighing | Resulting dry thickness | Origin on the work | Immediate corrective measure |
|---|---|---|---|
| Deficit greater than 20% of the prescribed mass | Lower than the required minimum thickness | Excessive spreading with the roller or uncompensated overly smooth substrate | Mandatory application of a third cross coat after complete drying |
| Compliance within plus or minus 5% of the prescribed mass | Compliant with certified dry film (generally 0.8 to 1.0 mm) | Rigorous compliance with the cross coat and tool notches | Validation of the substrate for tile installation after waiting time |
| Overconsumption greater than 35% of the prescribed mass | Significant local excess thickness (greater than 1.8 mm) | Accumulation in levelling compound hollows or overloads at corners | Mandatory extension of the drying time to avoid trapping water |
Treatment of thickness deviations and dry film management before bonding
Checking the thickness of liquid-applied waterproofing under tiles does not stop at the accounting record of empty buckets. When under-consumption is revealed by weighing, the tile-laying craftsman must restore the missing mass with an additional coat. This coat cannot be improvised: it must be applied in absolute compliance with the crossing rules relative to the previous pass. The technical gesture involves a perpendicular pass that saturates the micro-porosities and eliminates residual striations left by the roller or trowel. Conversely, the pitfall would consist in loading a single pass to make up for the deficit all at once, which would compromise the evaporation of the aqueous phase or solvents.
Before authorizing the application of tile adhesive, the foreman ensures that the entire surface exhibits homogeneous through-drying. Areas that required a catch-up pass require delaying the start of ceramic installation by an additional 12 to 24 hours depending on the ambient temperature and humidity. No destructive testing by cutting a sample is permitted on the finished work to measure the dry film: traceability by the weight of containers and wet film gauge readings constitute the only evidence admissible before site management.
Non-compliance of the material balance: catch-up protocols and traceability
When the material balance reveals under-consumption compared to technical data sheets and the requirements of standard SIA 248, the liquid waterproofing assembly no longer guarantees the required impermeability under tiles. The frequent temptation to mask the deficit with a levelling compound or to lay tiling directly constitutes a serious technical fault. If the empty containers do not correspond to the theoretical tonnage calculated for the treated surface, the membrane presents under-dosed areas vulnerable to water penetration. It is then out of the question to begin tile bonding.
- Note the deficit by weighing and surface calculationImmediately record the difference between the theoretical weight prescribed per square metre and the actual weight applied, deduced from the weighing of remaining buckets or opened packaging.
- Clean and prepare the intermediate filmIf the recoating time prescribed by the manufacturer is exceeded or if site dust has soiled the surface, carry out careful solvent-free dusting before any intervention.
- Apply an additional general cross coatApply a uniform third coat over the entire deck or partition concerned in order to exactly make up for the mass deficit, again respecting the cross directions.
In the event of localized excess with blistering or pronounced orange peel, the uncured zone must be mechanically scraped down to the sound substrate, then re-primed and retaken according to the complete system. Recording the consumed masses, batch numbers and controlled wet thicknesses in the site logbook protects the company against claims from site management upon acceptance of the work in accordance with standard SIA 248.
Frequently asked questions
What should be done if container weighing shows a lack of product even though the surface appears covered?
Visual opacity is misleading, because pigments mask the substrate from 0.2 millimetres onwards whereas standard SIA 248 and technical data sheets often require at least 1 millimetre dry. A shortage on the scale proves that the membrane is too thin. You must imperatively apply an additional cross coat over the entire area to reach the required grammage before any ceramic installation.
How to precisely measure the thickness of fresh liquid-applied waterproofing on the construction site?
Use a standardized comb gauge immediately after the passage of the roller or trowel. Firmly push the comb perpendicularly into the substrate until it touches the mortar or screed, then read the last wetted tooth. This wet thickness measurement makes it possible to correct the gesture without delay if the value lies below the fresh thickness prescribed by the technical documentation.
Why is it mandatory to apply waterproofing under tiles in two cross coats?
The first coat with a roller or trowel fills the micro-roughness of the substrate while inevitably creating grooves and micro-pores. The application of a second pass in the perpendicular direction crosses the film, closes residual porosities and guarantees regular thickness over the entire surface. This prevents any localized waterproofing defect, in accordance with the guidelines of standard SIA 248.
Can a dry thickness deficit be made up directly with tile adhesive?
No. Adhesive mortar provides no waterproofing function, even if it is classified as highly deformable or water-resistant. An adhesive applied to a membrane that is too thin suffers from water infiltration passing through tile joints in service. If the minimum dry thickness is not achieved during film control, only the application of a new coat of compliant waterproofing product is permitted.
Texts and standards cited
- SIA 248Installation of tiles and thin-slab coverings: liquid-applied waterproofing, admissible substrates and execution checks