Aller au contenu
Website
SIA 251 Tool 6.21 Online

Floating Screed Calculator (Cement / Anhydrite), Drying & Heating-Up (SIA 251)

Calculator for minimum thickness, drying time and the official heating-up protocol.

Interactive tool

Deadlines and protocol from the suissetec memo, values from the specifications. Heating start-up times (21 days for cement, 7 days for anhydrite), protocol “3 days at 25 °C, 4 days at maximum temperature” and screed bay table: extracts from SIA 251:2008 reproduced by a suissetec memo (paid standard not consulted). Thicknesses, drying, weight and CM moisture thresholds: specifications (the drying of 6,5 cm is 9 weeks by its own rule, not 6 to 8). The specifications' progressive protocol (+5 K per day) is offered as an option; the 10 K per day cool-down is an assumption of the tool.

A Thickness, volume, drying and residual moisture CM

m²
mm
mm

Thickness, quantities and moisture

Indicative minimum thickness
Volume of mortar to order
Weight of the screed
Waiting time before heating start-up
Natural drying
Maximum residual moisture

Volume = area × thickness × 1.05. Drying: 1 week per cm up to 4 cm, then 2 weeks per additional cm (rule of thumb, 20 °C and 50% relative humidity). The CM measurement with the carbide device is still to be done before laying the floor covering.

B Bay joints (screed bays)

m
m

Screed bays

Limits of SIA 251

Table 1 of SIA 251 according to the suissetec memo: cement with heating 6 m and 1.5 : 1; cement without heating 8 m and 2 : 1; anhydrite with heating 8 m and 1.5 : 1; anhydrite without heating no limit. The specification mentions 40 m² and 8 m: the standard is applied. Perimeter strip: 8 mm minimum, continuous.

C Heating start-up protocol, day by day

°C
days

Heating start-up calendar

Heating start-up calendar
DayDateFlow temperatureAction

Before the first heating-up, the flow temperature does not exceed 20 °C. For anhydrite, 50 °C at most. Heating-up does not replace site heating and does not prove that the screed has reached the CM laying threshold.

Embed this calculator on a website page

Paste this code into the page, or write [outil code="6.21"] in the content of a page on the site.

📄 File linked to this tool (free)

Move from calculation to full management

Keep your references at hand, then automate them in your quotes, bids and final statements.

⚡ Automate this calculation in our ERP / Soumission software (Trial)

Technical reference guide

SIA 251 standard (Floating screeds): minimum thicknesses and cover over underfloor heating pipes (CT vs Anhydrite CAF)

The SIA 251 standard floating screed thickness heating-up protocol (“Schwimmende Estriche im Innenbereich”, 2008 edition) sets the rules for a screed laid on a separating or insulating layer. On underfloor heating, the underfloor heating pipe cover 45 mm SIA 251 is the screed height above the pipes: at least 45 mm in cement screed (CT), i.e. 62 mm in total with 17 mm pipes, and 35 to 40 mm in anhydrite flowing screed (CAF), i.e. 52 to 57 mm in total.

Minimum thickness and waiting time before heating-up by binder
BinderPipe coverTotal thickness (17 mm pipes)Without heatingWaiting time before heating start-up
Cement screed (CT)at least 45 mmAt least 62 mm (standard 65 to 70 mm)at least 45 mm21 days
Anhydrite screed (CAF)35 to 40 mm52 to 57 mm35 mm (assumption)7 days

The drying time cement screed vs anhydrite CAF is calculated with the rule of thumb of one week per centimetre up to 4 cm, then two weeks per additional centimetre: 4 weeks for 4 cm, 6 for 5 cm, 9 for 6.5 cm and 10 for 7 cm, at 20 °C and 50% relative humidity. Drying also depends on the binder and on the ventilation of the room: the CM measurement remains decisive.

Note on the text of the standard. SIA 251 (paid) was not consulted. A Swiss technical sheet cites it for at least 45 mm in floating screed, increased by the outer diameter of the pipes in heated screed, which matches the 62 mm of the specification for cement. The 35 to 40 mm cover in anhydrite is that of the specification, not verified in the standard; the minimum thickness of an unheated anhydrite screed (35 mm) is an assumption of the tool. Discrepancy: the specification states “6 to 8 weeks” of drying for 6.5 cm; the rule it sets out gives 9 weeks, the value used by the tool. For the heating itself, see the heat pump and underfloor heating tool.

Why an anhydrite screed requires a residual moisture of ≤ 0.3% CM (versus 1.5% CM for cement screed)

The residual moisture CM carbide bomb screed is measured by taking a screed sample, which reacts with calcium carbide in a pressure vessel: the pressure of the gas formed gives the water content in % CM. Anhydrite screed is based on calcium sulphate, a binder sensitive to water: as long as it stays damp, it loses strength, and it must also be sanded on the surface before laying. The threshold is therefore very low: 0.3% CM with underfloor heating and 0.5% CM without, for all coverings. For cement screed, it is 2.0% CM without heating and 1.8% CM with heating for tiles, 1.8% CM without heating and 1.5% CM with heating for parquet, resilient floors and resins.

Maximum residual moisture (% CM) before laying the floor covering
SurfacingCement, without heatingCement, with heatingAnhydrite, without heatingAnhydrite, with heating
Tiles / natural stone2,01,80,50,3
Glued parquet / laminate1,81,50,50,3
Resilient floor PVC / linoleum / resin1,81,50,50,3

Note on the text of the standard. The title of this subsection contrasts 0.3% CM with 1.5% CM; the 1.5% CM threshold applies to cement screed only for parquet, resilient floors and resins with underfloor heating, the threshold for tiles being 1.8% CM. The cement thresholds for tiles (2.0 and 1.8) and those for anhydrite (0.5 and 0.3) are confirmed by a table of the German parquet association; the 1.8 and 1.5% CM for parquet, resilient floors and resins on cement are those of the specification, stricter than German sources (2.0 and 1.8), and not verified in Switzerland. The explanations on the binder (water sensitivity, sanding) are general principles, not taken from the standard. See also the tiling, parquet and resilient floors tools.

The heating-up protocol for a heated screed in Switzerland (7 or 21 day wait and temperature steps)

Heating-up of a screed may only begin 21 days after laying for cement screed and 7 days after laying for calcium sulphate (anhydrite) screed. Before this first heating-up, the flow temperature of the underfloor heating does not exceed 20 °C. According to SIA 251, as reproduced in a suissetec memo, the protocol holds 25 °C for 3 days, then the maximum flow temperature (the design temperature, 50 °C at most for anhydrite) for 4 days, then switches the heating off. A heating-up protocol, signed by the client and the contractor, records the procedure.

Heating-up schedule for a maximum temperature of 45 °C
DaySIA 251 protocol (suissetec memo)Progressive protocol of the specifications (+5 K per day)
Day 125 °C25 °C
Day 225 °C30 °C
Day 325 °C35 °C
Day 445 °C40 °C
Day 545 °C45 °C
Day 645 °C45 °C
Day 745 °C45 °C
Day 8stop45 °C
Day 9stop35 °C
Day 10stop25 °C

The specification's progressive protocol rises by 5 K per day from 25 °C up to the maximum temperature (40 to 45 °C), holds it for 4 to 7 days (4 days in the table), then steps back down: the calculator offers both protocols and a dated schedule. Heating-up does not replace site heating in cold weather and does not guarantee that the screed has reached the CM threshold: the floor-covering installer measures the moisture before laying.

Note on the text of the standard. The 5 K per day rise of the specification is not in the suissetec memo; manufacturers' protocols refer to the European standard EN 1264-4, without this 5 K step being confirmed there. The step-down is not quantified there, and the 10 K per day steps are an assumption of the tool. The memo's protocol is proposed by default. The 7 and 21 day periods are confirmed. The maximum flow temperature is also limited by the cantons' energy regulations (MoPEC): it must never be exceeded. The screed manufacturer prevails.

Contraction joints (40 m2 threshold and 8 m maximum length) and acoustic perimeter strip (SIA 181 / SIA 251)

The screed contraction joints 40 m2 divide the screed into bays, so that its shrinkage and expansion do not crack it. According to Table 1 of SIA 251 reproduced in the suissetec memo, the size of a bay depends on the binder and the underfloor heating:

Maximum size of a screed bay according to SIA 251
BinderWith underfloor heatingWithout underfloor heating
Cement (CT) 6 m side, ratio of 1.5 : 1 (square bay of 36 m² at most) 8 m side, ratio of 2.0 : 1 (square bay of 64 m² at most)
Anhydrite (CAF) 8 m side, ratio of 1.5 : 1 (square bay of 64 m² at most)no limit

For the screed in the example (140 m² of heated cement), at least 4 bays are needed; a 5.5 × 4.5 m bay respects the limit. Joints must also be provided at door thresholds and other narrowings of the floor, and at the boundary between a heated and an unheated zone.

The perimeter strip separates the floating screed from walls, door frames, columns and pipes: it provides impact sound insulation and lets the screed expand without stress. It is continuous, at least 8 mm thick, and rises above the finished floor covering. For noise, see the SIA 181 standard tool.

Note on the text of the standard. The title of this section, taken from the specification, speaks of a “40 m2 threshold” and a “maximum length of 8 m”. The SIA 251 table gives a 6 m side and a ratio of 1.5 : 1 for heated cement screed (36 m² for a square bay; a Sika technical sheet also gives 36 m² at most), and 8 m only for cement without heating (ratio 2 : 1) or heated anhydrite (ratio 1.5 : 1). The tool applies these limits, not the 40 m². The joint layout is drawn up by the architect: ⚡ Price your screeds in Soumission

Frequently Asked Questions on Screeds, Heating-Up and CM Moisture (FAQ)

1. What minimum thickness for a screed on underfloor heating: cement or anhydrite?

On underfloor heating, the screed must cover the pipes: at least 45 mm of cover in cement screed (CT), i.e. 62 mm in total with 17 mm pipes (the standard is 65 to 70 mm), and 35 to 40 mm in anhydrite flowing screed (CAF), i.e. 52 to 57 mm in total. A 65 mm screed on 17 mm pipes is therefore sufficient in cement, with 48 mm of cover.

A Swiss technical sheet cites the SIA 251 standard: at least 45 mm for a floating screed, increased by the outer diameter of the pipes in heated screed. The 35 to 40 mm cover in anhydrite is that of the specification, not verified in the standard (paid, not consulted): also follow the manufacturer's sheet.

2. How long to wait before heating a screed, and how does heating-up proceed?

Heating-up may only begin after 21 days for cement screed and 7 days for calcium sulphate (anhydrite) screed. According to the SIA 251 standard, as reproduced in a suissetec memo, the protocol is 3 days at 25 °C, then 4 days at the maximum flow temperature (45 °C in the example), i.e. 7 days, then stop; the flow temperature does not exceed 50 °C for anhydrite. The specification's progressive protocol (+5 K per day from 25 °C, hold, step-down in 10 K steps) lasts 10 days with the same values.

Heating-up does not guarantee that the screed has reached the moisture required for laying the floor covering: the CM measurement is still to be done. The 5 K per day rise is not in the memo and could not be confirmed elsewhere; the 10 K step-down stages are an assumption of the tool.

3. What residual moisture (% CM) before laying the floor covering, and how long does a screed take to dry?

For tiles, the threshold is 1.8% CM on heated cement screed (2.0% without heating); for parquet, a resilient floor or a resin, it is 1.5% CM with underfloor heating (1.8% without). On anhydrite screed, the threshold is 0.3% CM with underfloor heating, 0.5% without, for all coverings. Natural drying follows the rule of thumb of one week per centimetre up to 4 cm, then two weeks per additional centimetre: 9.0 weeks for 6.5 cm at 20 °C and 50% relative humidity.

The specification states “6 to 8 weeks” for 6.5 cm: the rule it sets out gives 9 weeks, the value used by the tool. The CM thresholds of 2.0 and 0.5 are confirmed by a table of the German parquet association; the values of 1.8 and 1.5% for parquet, resilient floors and resins are those of the specification, stricter than German sources (2.0 and 1.8), and not verified in Switzerland.

Indicative information drawn up from the tool's specification and a suissetec memo reproducing SIA 251:2008; it replaces neither the standard, nor the screed manufacturer's sheet, nor the heating designer.

📥 Ready-to-use pack · free

Download the document

The file is displayed on screen right away and we also send it to you by e-mail.

Your address is used to send you this file. See our privacy policy.