Key takeaways
- Systematic inspection of timber moisture upon delivery prevents major subsequent structural defects.
- Standard SIA 265 establishes the required equilibrium moisture content based on the purpose and exposure of the load-bearing element.
- The insulated-pin moisture meter measures the water content at the core of the timber piece.
- Rejection of a delivery is based on an accurate record and the duty to notify under the works contract.
Measuring the moisture content of timber upon receipt according to standard SIA 265
Delivery to the construction site constitutes the final stage at which the carpenter can reject non-compliant material without assuming liability for future defects. The residual moisture of the timber determines its shrinkage, dimensional stability, and the retention of mechanical stresses within the connections. Timber installed above the equilibrium moisture content will undergo in-service drying, leading to shrinkage cracks, twisting, and loosening of bolted or dowelled connections.
Standard SIA 265 specifies the equilibrium moisture content values of timber at installation according to the environmental climate of the structure. For timber frame structures located in enclosed and heated premises (service class 1), the target value is generally established at 10-12%, while it rises to 15% for covered but open structures (service class 2).
norme SIA 265
The reference tool on the construction site is the electrical resistance moisture meter with pin electrodes. Capacitive devices (non-destructive) only allow surface pre-scanning, but prove ineffective for assessing the moisture gradient at the core of heavy cross-sections.
- Selection of test piecesInspect at least 5 pieces per delivered batch, targeting primarily elements with heavy cross-sections or those located in the centre of the pack.
- Preparation of the pin moisture meterDrive in insulated pin electrodes (only the bare tip conducts current) to prevent surface condensation from distorting the core measurement.
- Positioning of the electrodesDrive the pins in parallel to the timber grain, at a minimum distance of 50 cm from the ends of the piece to avoid rapid drying zones through the end-grain.
- Driving to the reference depthDrive the pins to a depth equal to one-third of the thickness of the piece to obtain the actual average moisture value of the cross-section.
Formal rejection procedure and duty to notify upon delivery
When readings reveal that the tolerance thresholds permitted by standard SIA 265 or the specifications have been exceeded, the timber must not be unloaded or must be quarantined separately on the construction site. Accepting the material without written reservations releases the supplier from liability and draws the carpenter into the chain of consequential damage.
- Duty to notify (art. 365 CO)
- According to art. 365 CO, the contractor is liable for the good quality of the material supplied. If the material received from the supplier has a defect, the contractor must immediately inform the client in order to protect their rights and suspend installation.
| Structure purpose | Target moisture (standard SIA 265) | Maximum permitted tolerance | Required action on the construction site |
|---|---|---|---|
| Glued laminated timber (heated interior) | 10% | 12% | Standard acceptance if below 12%; rejection if above. |
| Timber frame (integrated insulation) | 12% | 15% | Strict inspection; rejection of the batch above 15%. |
| Traditional covered timber frame | 15% | 18% | Formal rejection above 18% due to risk of major shrinkage. |
| External structural timber (no ground contact) | 18% | 22% | Ventilated storage tolerated subject to drying before enclosure. |
The rejection notice must be formalized directly on the delivery note presented by the driver. The site foreman indicates the elements measured, the type of moisture meter used, the measurement depth, and the recorded values. They add the statement "Batch rejected for exceeding SIA 265 moisture tolerances" and obtain the driver's signature before the lorry departs.
On-site moisture measurement protocol and SIA 265 tolerances
Receiving structural timber on the construction site requires rigorous inspection as soon as the lorry is opened. Timber delivered with a moisture content higher than the intended equilibrium value causes structural deformations, shrinkage cracks, and defects in connections once the building is heated. According to standard SIA 265, the reference moisture content of structural timber must correspond to the future scope of use of the structure (service class).
Residual moisture is inspected using a pin moisture meter (electrical resistance measurement). Surface measurements using capacitive contact are not permitted for validating structural components: they only measure the surface skin of the timber and ignore the still-damp core.
- Sampling selectionCheck at least 5 pieces per delivered pack, distributed between the top, middle, and bottom of the bundle. On large solid timber components (KVH or glued laminated timber), check at least 10 points per batch.
- Measurement depthDrive the insulated pins of the drive-in electrode to a depth equal to one-third of the thickness of the timber piece (minimum 15 to 20 mm). Surface measurement is strictly prohibited.
- Positioning of the electrodesPlace the pins parallel to the timber grain, at least 50 cm from the ends of the piece to avoid end-drying zones.
- Temperature and species correctionAdjust the device according to the ambient temperature of the timber and the species (spruce/fir), or apply the correction chart provided by the instrument manufacturer.
| Service class | Environmental conditions | Equilibrium moisture content of timber | Max. moisture upon delivery |
|---|---|---|---|
| Class 1 | Enclosed and heated premises (e.g. interior framing) | 5% to 12% | 12% ± 2% |
| Class 2 | Covered unheated structures (e.g. timber roof structure under ventilated roof) | 12% to 20% | 15% ± 2% |
| Class 3 | Structures exposed to weather (e.g. bridges, walkways) | > 20% | 18% (glued laminated) / 20% (solid) |
Formal rejection procedure and immediate duty to notify
If measurements taken with the pin moisture meter exceed the values tolerated by standard SIA 265 or the specific provisions of the works contract, the carpenter must intervene immediately before full unloading or incorporating the timber into the structure. Accepting timber that is too wet without reservations transfers liability for future defects to the timber framing company.
The Swiss legal framework governs the carpenter's liability regarding the quality of materials installed. According to the Code of Obligations (CO), the contractor is liable for the good quality of materials supplied. Furthermore, pursuant to art. 365 CO, if the supplied material or technical conditions threaten to compromise the proper execution of the works, the contractor has a legal obligation to inform the client immediately (duty to notify), failing which they must bear the consequences of the defects.
- Formalise the measurement report: Record the batch number, instrument used, ambient temperature, pieces checked, and exact moisture contents recorded at the core.
- Take dated photographs: Capture the screen of the moisture meter driven into the piece with the bundle number clearly visible.
- Notify immediately in writing: Send the report to the supplier and site management, demanding replacement of the batch or the provision of a drying period in accordance with recognised trade practices.
- Halt installation: Prohibit the erection of non-compliant components to prevent any obstruction of drying once racking panels or vapour barriers are installed.
Managing moisture disputes upon delivery and formal rejection
Undetected residual moisture defects upon unloading constitute one of the most costly sources of claims in timber framing and timber construction. Introducing structural elements into the construction site in the form of solid timber, glued laminated timber, or cross-laminated timber with a moisture content above the tolerances established by standard SIA 265 inevitably causes major structural defects during in-service drying: differential shrinkage, grain splits, warping of components, and deformation of connections.
When the moisture measured with the pin moisture meter exceeds the target value defined for the projected service class, the site manager or foreman must immediately stop acceptance and issue a rejection of the goods. In accordance with the Code of Obligations (CO), a contractor who notes a defective supply or one unsuitable for the proper execution of the works must notify the client and the supplier without delay, failing which they must bear the direct consequences.
- Joint measurement and calibrationPerform measurements using an insulated-pin moisture meter driven to one-third of the timber thickness. Take at least three test points per piece across a representative sample of the batch in the presence of the lorry driver.
- Drafting the inspection reportRecord the measured values, ambient temperature, batch number, and time stamp immediately on the delivery note. Have the driver sign the document.
- Issuing the formal duty to notifyDraft a formal notice of delivery stoppage addressed to the supplier and the project manager, confirming rejection of the excessively wet batch or its storage pending expert assessment.
In the event of a dispute by the sawmill or manufacturer, the rejected pieces must be segregated from the rest of the site storage, kept under breathable tarpaulins protected from direct weather, and clearly marked. A joint expert re-inspection by oven-dry weighing or verification by a Lignum expert may be required to resolve the dispute prior to any refund or batch replacement.
Frequently asked questions
To what depth should the moisture meter pins be driven when receiving structural timber?
The insulated pins of the electrical resistance moisture meter must be driven perpendicularly to the grain to a depth equal to one-third of the thickness of the timber piece. This method ensures measurement of the core moisture of the material, avoiding errors related to surface drying or the presence of rainwater on the surface during transport.
What is the acceptable tolerance for residual moisture according to standard SIA 265 for framing timber?
Standard SIA 265 establishes the reference moisture content based on the intended service class. For framing timber incorporated in service class 1 (heated premises), the average residual moisture upon receipt must be 12%, with a strict tolerance of plus or minus 2%. Any exceedance exposes the structure to pronounced subsequent shrinkage.
What should be done if the lorry driver refuses to sign the moisture measurement report?
If the driver refuses to sign the measurement report, the foreman must state this explicitly on the delivery note along with the exact time. They immediately take clear photographs of the measurements displayed on the moisture meter inserted into the timber and forward the file to the site manager for formal notification to the supplier.
Can structural timber that is too wet be seasoned directly on the construction site?
Site drying is strongly discouraged for structural components. It occurs in an uncontrolled manner, causing severe drying cracks, irreversible warping, and delays on the construction site. Timber that does not comply with the requirements of standard SIA 265 must be rejected and returned to the factory for seasoning in a controlled kiln.
Texts and standards cited
- SIA 265Requirements and tolerances relating to residual moisture in structural timber.
- Code des obligations art. 365Immediate duty to notify from contractor to client in case of defective supplies or material.