Skip to content
Website
🧱 CFC 214Timber as a load-bearing material: species, grades and moistureChapter 3 of 10 in the section

Glulam: what to check at unloading and what causes downgrading

Upon truck arrival, the carpenter has only a few minutes to inspect massive timber elements before signing the delivery note. This chapter details the method for identifying critical defects in glued laminated timber, distinguishing shrinkage cracks from glue failures according to standard SIA 265, formulating unchallengeable reservations, and compiling a solid photographic record.

Key takeaways

  • Inspect faces and end-grain before complete unloading of timber framework components.
  • Distinguish drying checks from a delamination plane running through the glue line.
  • Immediately record precise, quantified defects on the carrier's delivery note.
  • Build a timestamped photographic record with a metric scale to prevent any subsequent dispute.

Critical defects in glulam and differentiation according to standard SIA 265

Unloading a ten-metre main girder requires immediate vigilance from the site foreman. As soon as the tarpaulin is removed on the lorry bed, visual inspection searches for geometric non-conformities, excessive moisture, and above all, loss of internal cohesion. A load-bearing member subjected to bending or transverse tensile stresses tolerates no adhesion defects between laminations.

Delamination
Physical separation of two consecutive laminations along the glue line, caused by inadequate gluing, insufficient factory clamping pressure, or sudden differential moisture uptake.

It is essential to distinguish between a mechanical shrinkage crack and a glue line separation. A shrinkage crack cuts through the wood grain perpendicularly or obliquely to the annual rings; it results from the natural desorption of the timber without severely impairing the shear plane if its dimensions remain within tolerances. In contrast, delamination strictly follows the glue line, revealing flat surfaces devoid of wood fibre tear-out.

Visual assessment criteria upon site acceptance
Type of defect observedNature of anomalyStructural consequenceDelivery decision
Shrinkage crack in timberRadial crack within a laminationSlight section reductionAcceptance under monitoring
Edge delaminationClear opening along the glue lineLoss of shear strengthRejection or blocking reservation
End split originating in glue lineDebonding at the beam endFailure of anchorage at supportsImmediate quarantine
Out-of-tolerance warpingAxial twist of the memberAssembly difficulty and stressesRejection for non-conformity

The presence of continuous debonding along a joint constitutes an immediate ground for downgrading the load-bearing member. In accordance with recognized engineering practices for timber structures under standard SIA 265, a structural member exhibiting a continuous glue-line failure loses its certified load-bearing capacity and must under no circumstances be installed in the structure.

Notification on delivery note and photographic evidence file

Discovering a defect on a glued laminated timber member requires an immediate administrative response. Signing a release without annotations extinguishes straightforward claims against the carrier and complicates legal recourse against the manufacturer. Pursuant to art. 367 CO, after delivery, the client inspects the state of the work as soon as feasible and notifies the contractor of defects. This diligence applies analogously to the carpenter's supplies.

  1. Geometric survey of the defectMeasure the crack length with a tape and insert a feeler gauge or thin steel rule to determine the exact depth of the opening.
  2. Bilateral recording on the receiptEnter the precise measurements on the carrier's paper copy or digital terminal, clearly identifying the member according to the assembly drawings.
  3. Contextualised overview photographTake a wide shot showing the girder on the trailer or under the crane, the lorry's registration plate, and the overall construction site surroundings.
  4. Macroscopic photograph with scalePhotograph the defect up close, placing an unfolded folding rule along the crack and the steel rule inserted into the delamination to prove the absence of bond.
  5. Immediate transmission to the technical officeSend the written notice and uncompressed digital files to the manufacturer and site management within the same half-day.

The photographic record forms the cornerstone of the statement of condition. Each image must include geolocation metadata and undeniable timestamping. To prevent any contractual dispute under art. 365 CO regarding the contractor's liability for materials supplied, operations on the disputed component must cease immediately. The girder remains stored flat on clean bearers, protected from the weather by a ventilated tarpaulin, pending formal appraisal by the timber engineer.

On-site technical diagnostics: distinguishing shrinkage checks from joint failures

When unloading a long-span glued laminated timber member, discovering a longitudinal discontinuity requires an immediate diagnosis before any craning or prolonged storage. The structural issue is determining whether the defect is merely superficial hygrometric shrinkage or a lack of adhesion between laminations, known as delamination. The latter directly impairs the transmission of longitudinal shear under bending loads according to the design criteria of standard SIA 265.

Criteria for distinguishing and accepting fissures in glulam
Observed characteristicShrinkage check (drying)Delamination (bonding defect)
Crack pathCrosses the wood grain, oblique or radial within a laminationStrictly follows the glue line parallel to the faces
Inspection of crack rootTorn wood fibres, presence of raw woody materialSmooth surface, visible vitrified glue or lack of adhesion
Position in cross-sectionFrequent at member ends or in the mid-height of side facesLocated exactly at the interface of two stacked laminations
Structural consequenceTolerable within defined opening and depth limitsRedhibitory: downgrading or rejection of load-bearing member

To characterise the defect, the team leader uses a metal feeler gauge (blade gauge from 0.1 mm to 1.0 mm) and a rigid straightedge. A shrinkage check shows irregular edges and wood fibre bridges across the bottom of the opening. Conversely, delamination produces a clean separation where the gauge penetrates to a continuous depth along the joint line without encountering resistance from wood fibres. This lack of cohesion indicates adhesive or cohesive failure of the resin, attributable to faulty pressing, exceeded open time, or incorrect moisture content during factory gluing.

Legal security, blocking, and non-conformity management

As soon as delamination or a through-crack is identified, unloading of the piece must be suspended or controlled to prevent further damage. The project manager or site foreman records the anomalies on the delivery note with millimetric accuracy: identification of the affected lamination from the soffit, exact defect length, maximum depth measured with the feeler gauge, and longitudinal location relative to the supports.

  1. Dimensional survey and loggingMeasure the opening, depth, and longitudinal extent of the separation. Record the explicit statement "refused due to joint delamination" or "piece quarantined subject to verification by timber engineer" on the carrier's paper copy or digital terminal before signing.
  2. Compiling the evidence fileTake a series of usable photographs including: an overview of the girder on the semi-trailer with its factory identification label, a mid-range view featuring an extended measuring tape along the defect, and clear close-ups showing the metal feeler gauge inserted into the glue line.
  3. Quarantine and technical blockingSet down the component on a level area, clear of the ground, on perfectly aligned timber bearers spaced every two to three metres to prevent any warping. Protect the element from weather using a ventilated tarpaulin that prevents greenhouse effects while stopping liquid water ingress into cracks.
  4. Formal notice to site management and supplierSend the complete photographic file and a copy of the signed delivery receipt via traceable mail. The contractor fulfils their duty of care by reporting the observed defect without delay, thereby freezing installation deadlines without incurring liability.

A contractor accepting delivery of a structural material remains liable for its conformity regarding the final works. The Code of Obligations (CO) explicitly stipulates in art. 365 CO that the contractor is responsible for the good quality of the materials they supply. Careful blocking of the member while awaiting an expert assessment and prohibiting any drilling or notching on a questionable element protects the company against any subsequent rejection of liability by the cutting or laminating plant.

Dispute management upon unloading: rejection, preservative storage, and notification

When the lorry arrives on the construction site and unloading reveals a major structural defect — such as distinct delamination or a continuous glue line separation — the technical decision must be made before the driver departs. Pursuant to art. 365 CO, the contractor is responsible for the good quality of materials they provide; if they discover a defect in materials, they must inform the client. The carpenter cannot allow a suspect beam to be installed under schedule pressure: a delaminated member loses its load-bearing capacity as defined by standard SIA 265 and directly compromises their liability as contractor.

  1. Immediate inspection and bilateral reservationRecord the written reservation on the delivery note prior to any signature. Describe the damage factually: "glulam beam no. 3, 10 m long, glue joint failure between laminations 4 and 5 over 2.80 m, installation refused". Have the driver countersign with their printed full name.
  2. Compiling the dated photographic dossierTake an overall photograph of the member on the flatbed or on the ground, followed by close-ups with a steel rule or depth gauge inserted into the opening, clearly showing the manufacturer's identification label and the timestamp.
  3. Decision to reject or arrange preservative storageIf the carrier leaves with the component, document its immediate return to the plant. If the beam is unloaded to release the truck, isolate it on timber bearers at least 150 mm high, clear of the ground, covered with a breathable tarpaulin, with a formal ban on lifting.
  4. Formal transmission and request for appraisalPromptly issue the notice of defects to the supplier by registered letter or receipted email, attaching the photographic dossier, demanding an inspection by the timber engineer or replacement of the member.

Frequently asked questions

How can you tell a shrinkage check from delamination with the naked eye?

A shrinkage check cuts across the wood grain and often stops when hitting growth rings or a knot. It features an irregular, fibrous root. Delamination or glue line opening strictly follows the bond line between two laminations in a completely straight path. A feeler gauge blade enters the delaminated joint without meeting any fibre resistance, indicating a bond failure deemed fatal.

What should be done if the driver refuses to sign the delivery note reservation?

If the driver refuses to initial alongside the text, explicitly write "driver refused to sign" on your retained copy and on theirs. Immediately take a clear photo of the member, the annotated note, and the lorry's registration plate on the construction site. Forward everything by email to the supplier and site management within the hour following unloading.

Can a ten-metre beam with slight splits be repaired on site?

A superficial drying check often remains permissible under standard SIA 265 if its depth does not compromise shear performance. Conversely, for glue line delamination, no repair using screws or resin injection may be improvised without structural calculations approved by the civil engineer responsible for the works and written consent from the manufacturer guaranteeing the required strength class.

What blocking conditions apply when storing a rejected beam?

Place the member on a level area, on dry timber bearers at least 100 to 150 millimetres high to halt rising damp. Bearers must be spaced no more than two to three metres apart to prevent residual sag. Protect the member with a waterproof tarpaulin ventilated on its underside, avoiding direct contact with the upper faces, while awaiting the joint inspection by appointed experts.

Texts and standards cited

  • SIA 265Timber structures - Rules for structural design and evaluation
  • CO art. 365Materials and building ground: the contractor is liable for the sound quality of materials they provide; if material provided by the client or ground designated by them is found defective, or if another circumstance jeopardises the proper or punctual completion of the work, they must immediately inform the client, under penalty of bearing the consequences (para. 3).

In the same section