Skip to content
Website
🧱 CFC 214Cross-laminated timber (CLT): panels, lifting and jointsChapter 7 of 10 in the section

CLT and Fire Protection: Encapsulating or Leaving Timber Exposed

This chapter helps decide between encapsulation and exposed timber to satisfy fire resistance requirements. You will learn how to calculate the impact of charring rate on the residual load-bearing section, incorporate this margin into ordered CLT thicknesses, and coordinate installation on the construction site in compliance with VKF fire protection regulations.

Key takeaways

  • Board encapsulation protects the timber and avoids structural oversizing of CLT panels.
  • Leaving the timber exposed requires a sacrificial cross-section calculated according to the standard charring rate.
  • The required fire resistance directly determines the number and thickness of the panel plies.
  • Premature delamination of glued plies under fire conditions governs the thickness ordered from the manufacturer.

Deciding Between Protective Cladding and Controlled Combustion of CLT

In Swiss timber construction, structural design to meet fire resistance requirements is based on two distinct approaches: full encapsulation of the load-bearing element or the calculation of a sacrificial cross-section leaving the material surface visible. The fire protection regulations of the Association of Cantonal Fire Insurers (VKF) define the performance required for walls and floors, often expressed as criteria REI 30, REI 60, or higher depending on the occupancy and geometry of the building.

Encapsulation
Passive protection of a structural timber element using a continuous non-combustible lining, delaying or preventing the heating, ignition, and charring of the substrate for a standardised duration.

Board encapsulation, generally achieved using specific fire-rated plasterboard or fibre-reinforced gypsum boards, allows the CLT panel to be kept at its ambient temperature structural sizing. The role of the thermal screen consists in keeping the timber temperature below the critical pyrolysis threshold for the prescribed regulatory duration. For the carpenter, this method reduces the volumes of raw timber to be ordered from the timber framer or laminator, but shifts a significant share of labour to installation on the construction site or in the prefabrication workshop, whilst requiring rigorous air-tightness at panel junctions to block hot gases.

Conversely, leaving the timber exposed responds to strong architectural choices, but transfers the protective effort directly into the bulk of the CLT panel. Without a protective screen, the exposed face is subjected to direct flame action. The material then burns in a predictable manner, creating a superficial char layer that insulates the core of the panel. The sizing must then incorporate an extra thickness of consumed material that no longer contributes to taking up static loads in a fire situation.

Determining the Sacrificial Cross-Section and its Consequences for Ordering

To size a CLT panel left visible in a fire situation, the design office applies a standard one-dimensional charring rate. According to the timber structural calculation standards recognised in Switzerland, this rate is commonly assumed to be around 0.65 mm per minute for solid softwoods, but must be increased for cross-laminated timber due to the specific behaviour of glue lines.

Theoretical thickness loss per exposed face according to the required resistance duration
Required performanceTheoretical charring rateGross sacrificial thicknessThermal transition layerEstimated total loss
REI 300.65 mm/min19.5 mm7.0 mmapprox. 27 mm
REI 600.65 to 0.80 mm/min39.0 to 48.0 mm7.0 mmapprox. 46 to 55 mm
REI 900.80 mm/min (with delamination)72.0 mm7.0 mmapprox. 79 mm

The critical phenomenon in CLT is thermal delamination. When the charred outer layer detaches due to the degradation of the adhesive under high temperature, the underlying ply is suddenly exposed to direct fire without the protection of the residual char layer. This detachment locally accelerates the combustion rate. The site foreman must ensure that the type of bonding used by the CLT manufacturer guarantees high-temperature performance to prevent this premature falling-off of charred plies.

The consequence for the ordered thickness is direct and substantial. For a floor slab that must provide REI 60 performance on an exposed soffit, the usable thickness loss commonly exceeds 50 mm. A panel whose ambient temperature statics would require a standard five-ply build-up of 140 mm (for example 30-20-40-20-30 mm) must often be ordered in seven plies or with significantly thickened lower plies, reaching 180 mm or even 200 mm in total thickness. This extra material cost is accompanied by an increase in dead weight of around 20 to 30 kg per square metre, which alters the loads on hoisting equipment and bearing reactions on load-bearing walls.

On a contractual level, according to art. 365 CO, the contractor is liable for the good quality of the material supplied. If the client demands exposed timber during the works whereas the initial sizing planned for board encapsulation, the carpenter must immediately report the technical incompatibility. Ordering panels with the initial thicknesses without verifying the residual cross-section would compromise the structural safety of the building in the event of a fire incident.

Installation of Board Encapsulation and Management of Junctions

When a structure requires increased fire resistance without extra thickness of solid timber, board encapsulation provides the direct technical alternative to free combustion. In Swiss practice, this passive protection aims to delay the heating of the cross-laminated timber load-bearing panel using a non-combustible or low-combustibility lining, generally composed of specific fire-rated plasterboard or mineral-fibre-reinforced gypsum boards.

Encapsulation (K protection)
The ability of an internal lining (for example fire-rated plasterboard) to protect the underlying timber structure against ignition and charring for a defined standard period (generally K 30 or K 60 according to VKF fire protection directives).

For the carpenter, successful encapsulation relies not only on the type of boards, but also on strict adherence to mechanical fixing and joint sealing. Screws must pass through the cladding layers to anchor into the first layer of solid timber with an embedment depth conforming to the board manufacturers' approvals. When the requirement reaches EI 60 or REI 60 under protection, installation is most often carried out in two staggered layers with offset joints. All board joints, screw heads, and corner junctions must be filled with an approved firestop sealant.

On floor or roof slabs, direct fixing of boards onto the CLT optimises clear ceiling height. However, if building service runs pass under the floor, the substructure made of metal sections or timber battens must incorporate non-combustible mineral insulation (rock wool with a melting point above 1000 °C) to prevent any hot spots under the underside of the load-bearing panel.

Techno-Economic Appraisal: Consequences on Ordered Thickness

The choice between leaving the timber exposed or encapsulating the CLT directly impacts the industrial order placed with the panel manufacturer. In the case of exposed timber, taking the sacrificial cross-section into account requires ordering a gross thickness that includes the charring margin, the thermal transition layer, and the residual structural reserve in fire conditions. For a floor subject to an REI 60 requirement, this commonly results in shifting from a standard 5-ply 140 mm panel to a reinforced 160 mm or even 180 mm panel.

Comparison of Construction Site Impact Between Exposed CLT and Encapsulated CLT
Construction site criterionExposed CLT option (sacrificial section)Encapsulated CLT option (board protection)
CLT panel thicknessIncreased (e.g. +20 to +40 mm to compensate for pyrolysis)Optimised according to ambient temperature statics alone
Ordered surface qualityVisible industrial or living-space quality (sanded, selected)Non-visible / standard quality (economical)
Dead weight of elementsHigher, increasing permanent loads and crane tonnageLower for the bare panel, but weight of boards to be added to finishing work
Finishing work interfaceNone at the ceiling (finished timber), increased vigilance regarding construction site soilingInvolvement of board installers, filling, sanding, and painting
Protection of connectorsComplex rebates, concealed steel brackets, and mandatory timber plugsStandard metal connectors protected beneath the lining

Leaving the timber exposed also imposes requirements on connection details. Connection brackets, angle plates, and fixing screws must be fully recessed or hidden under timber trims or timber plugs with a thickness equivalent to the charring layer. Conversely, encapsulation permits the use of visible connectors installed on the surface of the CLT, as the boards provide the thermal screen required by the fire resistance requirements of the structure.

During the tender phase, the extra supply cost of thicker, visual-grade CLT (often in the range of 30 to 60 CHF more per square metre of raw panel compared to a non-increased non-visual grade) must be weighed against the firestop board lining item within the finishing work. In terms of responsibilities, in accordance with art. 365 CO, the contractor notifies the client of any discrepancy between the working drawings, the desired finished appearance, and the target fire resistance class before starting factory fabrication.

Managing Order Discrepancies and Interface Disputes During Assembly

On the construction site, disputes frequently arise when the delivered cross-laminated timber panel does not match the option selected when awarding the contract: undersized panel for exposed timber or encapsulation recesses omitted at the supports. If the fire resistance requirement of the building specifies an REI 60 rating and the ordered thickness does not include the sacrificial cross-section required by the fire protection concept, the element cannot be left bare. The carpenter must then refuse technical acceptance of the panel or formally record the non-conformity before any hoisting.

When the order was placed without incorporating the charring extra thickness for a surface intended to be left exposed by the architect, two remedial routes exist at the shop drawing stage. The first consists in recalculating the structure under fire conditions with the timber engineer to check whether the actual load ratio of the element allows a sufficient residual margin. If the structural justification fails, the second route requires board encapsulation using standard or fire-rated plasterboards with direct mechanical fixing onto the CLT plies. This change causes a loss of internal headroom and alters the finished levels of slabs and wall junctions.

The site foreman systematically formalises the agreement between the fire quality assurance manager (VKF), the timber engineer, and the site management via a written addendum. This protocol establishes the new total thickness, screw centres for the lining to prevent premature shear under thermal stress, and the financial breakdown for hardware adjustments.

Frequently asked questions

Can a CLT panel be ground down locally to correct a plumbness issue beneath encapsulation?

No. Even when intended to be covered with fire-rated plasterboard, the CLT panel has a load-bearing outer ply whose minimum thickness was included in the structural calculation report. Notching or grinding this ply weakens the mechanical strength of the element and compromises the anchoring of the protective lining fixings. Any adjustment must be carried out using shims beneath a secondary sub-frame following agreement from the timber engineer.

What should be done if the engineer suddenly requires leaving a panel sized for encapsulation exposed?

You must refuse the removal of the lining without a revision of the structural calculations. A panel designed for encapsulation features an optimised thickness without sacrificial extra thickness. Leaving the timber exposed reduces the residual cross-section under the effect of charring during a fire. Without a validated thermal recalculation or the addition of an approved intumescent coating under a specialist contract, the compliance of the works with VKF directives is no longer guaranteed.

How should CLT fixing screw heads be treated if the panel remains exposed with REI 60?

Unprotected metal connectors rapidly transmit heat to the core of the timber. In an exposed configuration with a sacrificial cross-section, two options are recognised: countersinking the screw heads into a rebate sealed with a timber plug of equivalent thickness to the calculated charring layer, or justifying the screws according to the fire annex of specific SIA standards by applying certified cover pieces.

What are the consequences for accessory orders if a CLT ceiling switches from exposed to encapsulated?

This change alters service penetrations and technical interfaces. Adding one or two plasterboards thickens the finished build-up by 15 to 30 mm, which lengthens hangers, changes the length of through-fixing screws, and shifts bearing levels on walls. Cutting lists must be adjusted immediately to order connectors suited to this new dimension.

Texts and standards cited

  • CO art. 365material and site: the contractor is liable for the good quality of the material supplied; if the material supplied by the client or the site designated by him proves defective, or if any other circumstance compromises the regular or punctual execution of the work, he shall immediately inform the client, failing which he shall bear the consequences (para. 3).
  • LAA art. 82general rules of prevention: to prevent occupational accidents and illnesses, the employer takes all measures shown by experience to be necessary, feasible using the state of the art, and adapted to the given conditions; workers assist him (in particular, they use personal protective equipment).

In the same section