🧱 CFC 214Cross-laminated timber (CLT): panels, lifting and jointsChapter 6 of 10 in the section

Visible face CLT: ordered surface quality and protection until acceptance

This chapter details the management of cross-laminated timber with an exposed face, from the contractual definition of the facing to the acceptance report. You will learn to lock in appearance requirements, deploy suitable workshop and assembly protections, and organise site demobilisation without damaging machined raw surfaces.

Key takeaways

  • The order must imperatively specify the appearance face according to the criteria defined in the enterprise contract.
  • Any footprint, standing water or tannin permanently penetrates open fibres.
  • Protective films applied in the factory require strict checking during offloading on the construction site.
  • Immediate joint acceptance avoids damage caused by other trades being attributed to the timber contractor.

Ordering surface quality and securing factory protection

Structural cross-laminated timber (CLT) is not treated like a simple structural work element when one or more faces remain visible in the finished work. A visible face requires rigorous selection of the outer laminations, free from open resin pockets, loose black knots or fungal discolouration. The order placed with the manufacturer must make the distinction explicit between non-visible industrial quality, standard visible quality and superior visible quality. If this clarification is missing from the contractual documents, the element is delivered to the basic production standard, rendering any subsequent rejection unjustifiable.

Distinction criteria for CLT facings according to use
Appearance classUse of the elementSurface tolerancesRequired factory protection
Industrial (NVI)Lined partitions, floors under screedLoose knots permitted, bluestain tolerated, no filler appliedBasic transport sheeting
Standard visible (VI)Offices, dwellings, common exposed soffitsSound intergrown knots, filled splits, calibrated grit sandingWaterproof peelable film applied in the factory
Superior visible (SI)Prestige projects, primary decorative partitionsLaminations sorted for aesthetic grade, no black knots, homogeneous grainIndividual waterproof wrapping and edge protection

As soon as shop drawings are issued, the carpenter identifies the high-grade face on each element using clear conventional marking. Protection begins at the factory: in-line application of a peelable self-adhesive film, permeable to water vapour but impermeable to liquids, guarantees facing integrity against splashes. This measure protects panels during road transport and crane offloading operations, preserving the original shade against greying caused by light oxidation.

Preserving facings on the construction site and achieving acceptance

Once installed, visible cross-laminated timber becomes the prime target for construction site damage. Safety shoe soles caked in calcareous mud, power tool fluids, or metallic oxidation runs deeply mark the material. Cross-cut wood fibres or surface plies absorb these impurities by capillary action. Subsequent sanding on the construction site remains an illusion: localised abrasive mechanical action hollows the facing, breaks flatness under raking light and highlights grain differences visible to the naked eye.

  1. Installing mechanical overlay protection on the floorOn floor slabs visible on their soffits or intended to remain bare, deploy hardboard panels or breathable felts as soon as installation is complete to prevent any direct contact with footwear soles.
  2. Managing weather-related water ingressImmediately sweep away rainwater puddles forming on panels before water enters butt joints or runs down exposed underside faces.
  3. Awareness and demarcation of visible areasMark high-appearance partitions with signs prohibiting notices or direct writing with greasy carpenter's pencil, chalk or felt-tip pen.
  4. Final cleaning and film removalRemove peelable films only before the acceptance inspection, dusting surfaces using industrial vacuum cleaning without pressurised water jets.

The contractor carrying out the timber work must inform the site management immediately if an external circumstance threatens the work, in accordance with the general principle of art. 365 CO. As soon as structural assembly is complete, carrying out a joint inspection record of visible surfaces formally delimits the carpenter's liability before finishing work trades intervene, avoiding the unjustified attribution of subsequent impacts, plaster runs or formwork oil marks.

Construction site marks and impossible touch-ups: the reality of visible CLT

On a cross-laminated timber structural site, the idea that a final pass with a sander will erase accumulated dirt is an illusion. The outer plies of a CLT panel machined to visible quality have a calibrated finished thickness, generally factory-planed. Aggressive sanding on the construction site destroys local flatness, hollows out the wood grain, exposes glue lines between laminations and creates a matt area that stands out starkly under raking light.

Certain mechanical and chemical aggressions penetrate deep into the sapwood or react with lignin. A construction site boot sole soiled with mud or cement dust crushes surface fibres while embedding alkaline particles into them. Worse still, metallic residue from rebar grinding or threaded rod cutting oxidises at the slightest moisture: it causes blue-black iron-tannate stains that penetrate several millimetres into the wood.

Impact of construction site contamination on visible CLT panels and limits of remediation
Type of aggressionAlteration mechanismFeasibility of touch-upMandatory preventive measure
Cement dust / laitanceAlkaline reaction, irreversible greyish or brownish shift under waterVery light sanding if dry, impossible after rehydrationImmediate dry vacuuming, damp sweeping prohibited
Metal grinding filingsFerric oxidation upon contact with tannins, indelible black spottingNo neat local touch-up without hollowing out the faceWaterproof sheeting or strict ban on grinding nearby
Boot prints / soilMechanical crushing of surface fibres and ingressFine-grit sanding (120-150) with risk of haloingWorkshop overshoes or preserved peelable films
Dirty water runs / tanninsMigration of dried impurities creating dark water ringsNeutralising wash highly unpredictable, visible shade differenceKeep sheltered from rain and clear standing water immediately

When the specifications mandate an industrial or living-space appearance quality, the only viable policy for the assembly crew remains the absolute avoidance of direct contact with structural work pollutants. Any damage observed on an installed load-bearing element falls under immediate notification mechanisms within the meaning of art. 365 CO, failing which the carpenter's liability may be engaged for the aesthetic depreciation of the finished work.

Final cleaning, joint inspection record and acceptance of the facing

The preparation phase for acceptance begins as soon as the building envelope is permanently closed. Temporary protections fitted at the factory or on the construction site must not be removed prematurely: as long as finishing work trades move across CLT floors or work alongside visible partitions, the protective film remains in place. It is removed room by room, just before the inspection of surface conditions.

The final construction cleaning protocol is limited to non-invasive manual procedures. All high-pressure cleaners or general water spraying are prohibited. Dust removal is carried out using an industrial vacuum cleaner equipped with a soft brush to avoid scratching soft timber. Adhesive residue from tapes or airtightness strips is dissolved using a cleaner specifically formulated for softwoods, applied with a clean, lint-free cloth, without rubbing vigorously to avoid burnishing the surface.

  1. Methodical removal of peelable filmsRemove perimeter protective strips and surface films with a steady motion, without running a metal blade directly over the timber, to avoid scoring the visible facing.
  2. Complete dry vacuumingRemove sawing dust, plaster and mineral particles with a soft vacuum brush before applying any liquid or cleaning agent.
  3. Spot degreasing and adhesive removalTreat adhesive residues, strap marks or assembly markings with a mild wood-safe solvent, followed immediately by wiping with a dry cloth.
  4. Appearance review under service lightingVisually inspect panels from the standard distance and under the lighting planned for room operation, without casting artificial raking light that does not comply with standards.

The client examines the work as soon as feasible according to the rules of standard SIA 118 and federal law. Diligently drawing up a joint inspection record with high-definition photographs protects the carpenter against late claims, which are common during subsequent interior fit-out phases when painters, electricians and screeders work in the immediate vicinity of cross-laminated timber elements.

Managing facing non-conformities and contractual remedies

On a cross-laminated timber construction site left visible, deterioration of a high-grade surface immediately turns a structural element into an aesthetic dispute. The technical impossibility of localised sanding without creating a hollow or a difference in sheen forces the installation team to manage liabilities strictly. As soon as damage caused by bad weather, soiled footprints or the intervention of another trade appears, strict compliance with contractual procedures takes precedence over any attempt at improvisation.

In accordance with art. 365 CO, if any circumstance compromises the regular or timely execution of the work, the contractor must inform the client. This formal notification must establish the facts immediately upon offloading or after third-party contractors have accessed protected floors. Under standard SIA 118, a notice of defects or an entry in the site logbook establishes causation before facings suffer cumulative damage.

  1. Immediate joint inspection recordProduce an accurate photographic survey referenced to the layout drawing as soon as fouling or water damage is identified, in the presence of the site management.
  2. Timber moisture content measurementCheck moisture content using insulated pins to record whether the panel has suffered deep wetting likely to cause bluestain under the film.
  3. Selection of the corrective measureConfirm in writing with the architect whether to apply an opaque wood stain, carry out uniform mechanical de-nibbing across the entire bay, or accept a price reduction under CO.

If the client rejects the panel invoking CO, rights in the event of defects allow for remediation, price reduction or contract cancellation. For visible CLT, replacing a load-bearing panel already integrated into the structure often proves technically disproportionate. Negotiations then lead to financial compensation or non-load-bearing internal lining, the interface costs of which must be thoroughly documented for final settlement.

Frequently asked questions

Can a water ring on visible CLT be corrected by sanding on the construction site?

No. Water causes tannins to rise and deeply swells fibres in the outer softwood ply. Localised sanding with an orbital sander hollows the wood and alters local flatness. Under raking light, this depression remains instantly visible. The only acceptable measure is very light, uniform de-nibbing across the entire surface of the panel, followed by the application of an equalising pigmented finish.

Who is responsible for protecting visible CLT slabs after lifting?

The carpenter provides and installs the initial protection for their elements. However, custody of the works and the maintenance of protections against damage from finishing work trades fall under construction site coordination. Once floors are handed over compliant and recorded under standard SIA 118, intervening contractors answer for mechanical damage and fouling they cause directly to the protective films.

How should construction adhesive residue be removed from a raw facing?

Adhesive tapes not designed for wood surfaces leave glue residues that polymerise under ultraviolet light. Strong chemical solvents must not be used because they cause local discolouration of the timber or leave indelible oily marks. Gentle mechanical rubbing using a specific cleaning block or neutral, citrus-based cleaning agents pre-tested on an offcut from the same batch should be used instead.

What should be done if the visible CLT package shows defects upon opening the packs?

Installation of the affected element must be halted and the defect recorded on the carrier's delivery note. Notify the supplier and site management of the issue through a formal notice with supporting photographs before any permanent fixing. Installing a defective panel constitutes tacit acceptance of the material, making it very difficult to backcharge remediation costs to the cross-laminated timber manufacturer later.

Texts and standards cited

  • CO art. 365material and site: the contractor is liable for the sound quality of the material supplied; if the material supplied by the client or the ground designated by the client is found to be defective, or if any other circumstance compromises the regular or timely execution of the work, the contractor shall immediately inform the client, under penalty of bearing the consequences (para. 3)
  • COclient's rights in case of defects in the work: rejection, price reduction, remediation, damages; any clause agreed in advance restricting or excluding the right to defect remediation is void if the defect relates to a structure (para. 2bis, since 1 January 2026)
  • norme SIA 118General conditions for construction work