🧱 CFC 283Moisture in timber and in the roomChapter 2 of 10 in the section

Wood moisture content: delivery rate, equilibrium moisture content and core measurement

Hygrometric control upon delivery protects the flooring installer against major defects caused by the dimensional shrinkage of wood. After this chapter, you will know how to determine the expected equilibrium moisture content in the room in accordance with SIA 253, check the moisture content of packages without needlessly tearing open the packaging, and master measurement by electrical resistance or capacitance methods on your solid and engineered parquet elements.

Key takeaways

  • Moisture control is carried out upon receipt, before any widespread unpacking of packages on the construction site.
  • Standard SIA 253 sets a moisture content at delivery generally between eight and ten percent.
  • Wood delivered with too high a moisture content will undergo inevitable shrinkage, causing cracks and open joints in service.
  • The electrical moisture meter with calibrated pins remains the standard construction site device compared to oven weighing.

Delivery moisture content and hygrometric equilibrium: anticipating shrinkage in heated environments

Wood is a hygroscopic material whose dimensions vary continuously depending on moisture exchange with the ambient air. When a batch of parquet is delivered to the construction site with a water content higher than the equilibrium moisture content of the building in service, the desorption phenomenon starts as soon as the heating is turned on. This loss of moisture causes marked transverse shrinkage of the boards. The aesthetic and structural consequences appear within a few weeks: widespread opening of edge joints, end-cracking of boards, and cupping of glued solid parquet. Each point of moisture lost below the fibre saturation point results in measurable shrinkage: on European oak, a 3% loss in moisture equates to a reduction of approximately 0.8 mm per 120 mm wide board. To prevent these failures, the flooring installer must compare the moisture content of the delivered boards with the service conditions defined by standard SIA 253.

In contemporary housing in Switzerland, characterised by airtight thermal envelopes and underfloor heating systems, the relative air humidity regularly drops between 30% and 45% during the winter for an indoor temperature of 20 °C. In such an environment, the equilibrium moisture content of wood stabilises between 6.5% and 8.5%. Parquet delivered at 11% will inevitably undergo severe drying once installed. Standard SIA 253 sets the permissible range at delivery between 7% and 11% depending on the parquet type and installation method, recommending a target value of 9% for solid wood elements and 8% for multi-layer parquet installed on heated floors.

Equilibrium moisture content of wood according to ambient room climate
Indoor temperatureRelative air humidityEquilibrium moisture content of oakPredictable dimensional behaviour
20 °C35% (dry winter)7.0%Strong shrinkage with joint opening if wood is delivered above 9%
20 °C50% (mid-season)9.3%Stable equilibrium and maintenance of factory machining dimensions
22 °C65% (humid summer)11.8%Moderate swelling absorbed by peripheral expansion gaps

Board measurement protocols: pin-type moisture meter and reference weighing

Qualitative acceptance of parquet requires immediate hygrometric checks before general opening of the pallets. The flooring installer carries out surveys by cleanly cutting the protective plastic on several packages distributed in the centre and periphery of the pallets. The surface capacitance moisture meter allows non-destructive preliminary sorting, but the electrical resistance measurement with insulated pins remains the reference method on site to probe the core of the wood, while the gravimetric oven method constitutes the legal arbitration recourse.

  1. Device setupSelect the compensation curve for the wood species in question and calibrate the device according to the core temperature measured in the package.
  2. Insertion of insulated electrodesDrive the pins perpendicular to the wood fibres. The insulated sheath of the pins ensures a measurement free from surface disturbances. On solid parquet, drive the pins to one-third of the thickness to measure the average moisture content.
  3. Multiplying readingsTake at least three measurements per tested board: one in the central area and two at approximately 100 millimetres from the ends, in order to detect an internal moisture gradient.
  4. Recording valuesImmediately record the percentages measured, manufacturing references, and room climate on the joint inspection record for receipt.
Weighing and oven-drying method
Reference gravimetric method consisting of weighing a wood sample immediately after extraction, drying it in a ventilated oven at 103 °C until constant mass is reached, and then calculating the mass ratio of water to anhydrous wood.

Installing non-compliant material transfers full liability for subsequent cracks and uneven levels to the installation company. The mere mention of conformity on the delivery note does not exempt the flooring installer from their incoming technical check. By rigorously tracking these measurements before any unpacking, the team protects its work against claims related to hygrometric deformations in service.

Site receipt inspection and sampling under packaging

Unloading parquet packages is a decisive step for the flooring installer. As soon as the pallets are accepted and stored on the structure, the burden of proof in the event of a subsequent dispute becomes particularly difficult to establish. In accordance with the rules of standard SIA 253, wood moisture control is carried out upon arrival on the construction site, imperatively before the general opening of sealed packages. The delivered material must correspond to the order and the anticipated equilibrium climate in the completed building. Factory packaging protects the wood against bad weather during transport; splitting or opening them prematurely in a still damp room exposes the boards to rapid water vapour reabsorption, invalidating any joint inspection record.

  1. Visual inspection and condition of coveringsCheck for the absence of wetting traces on the pallets. Inspect the polyethylene films: any tear, perforation, or sign of condensation under the plastic requires an immediate note on the carrier's consignment note.
  2. Differential thermal readingRecord the surface temperature of the wood and the room air temperature using an infrared thermometer. If the wood arrives cold in the winter season, let it temper in its sealed wrapper to prevent any surface condensation before measurement.
  3. Electrical resistance surveySelect three packages at random per 50 m² section at the core of the pallets. Locally cut the packaging to insert the insulated electrodes at one-third of the board thickness, parallel to the grain, then reseal the cut with technical adhesive tape.
  4. Drafting the delivery recordRecord the measured moisture values (individual and average values), factory batch numbers, as well as the room temperature and relative humidity on the joint inspection receipt sheet.

Batch decision: calculation of predictable shrinkage and management of discrepancies

A wood delivery whose mass moisture content exceeds contractual tolerances generates severe mechanical stresses upon the first heating cycle. Under the Swiss winter indoor climate, ambient air frequently drops to 30 or 35% relative humidity, driving the boards towards a hygrometric equilibrium of 6 to 7%. Solid oak parquet delivered at 11% moisture will inevitably undergo marked transverse dimensional shrinkage. For a board 140 mm wide, such an imbalance results in a joint opening close to one millimetre between each row, degrading flatness and shearing the elastic adhesive beads applied to the screed.

Decision matrix according to moisture measured on boards at delivery
Measured moisture contentDeviation from local equilibrium (8 to 9%)Predictable behaviour of parquetSite measure to be applied
Below 7%Pronounced water deficitSummer swelling, risk of bucklingBatch rejection or controlled buffer storage
7% to 9%Compliant with standard SIA 253 tolerancesOptimal dimensional stability in serviceReceipt accepted, installation authorised on dry substrate
10% to 11%Moderate excess (1 to 2% above)Winter shrinkage, clear joint openingAnomaly notice, quarantine under film
Above 11%Critical non-conformityMassive shrinkage, wood cracking and debondingImmediate rejection with recorded carrier return

If the inspection highlights non-conformity before unpacking, the team leader immediately informs the site management and the supplier via a formal written notice. Pursuant to the general provisions of the Code of Obligations governing works contracts, prompt reporting of material defects releases the installer from any liability regarding subsequent hygrometric defects. Attempting to artificially dry a batch that is too wet directly on the construction site represents a major technical error: sudden temperature changes generate irreversible internal stresses causing warping and surface cracks on the boards.

Action to be taken in case of hygrometric non-conformity of the delivered batch

When the receipt inspection reveals a wood moisture content higher than the tolerances provided for the construction site, the flooring installer must imperatively stop installation. A parquet board delivered at 11% or 12% mass moisture, destined for a new building whose equilibrium moisture content during the winter period will establish itself around 7% to 8%, will inevitably undergo significant dimensional shrinkage once the heating is in service. This transverse shrinkage will result in the appearance of shrinkage cracks, edge gaping, and the potential rupture of certain adhesive beads.

  1. Immediate quarantine of palletsLeave packages closed under their original waterproof plastic film. Unpacking packages that are too wet in a building undergoing drying exacerbates moisture reabsorption or causes erratic surface drying of the boards, leading to cupping and geometric deformations.
  2. Drafting the joint inspection recordMeasure several representative boards on different packages using the electrical moisture meter with insulated pins or by weighing after oven-drying. Record the values, room temperature, relative air humidity, and batch numbers on the construction site report.
  3. Written notification to the supplier and site managementForward the report without delay, citing non-conformity in accordance with standard SIA 253. According to the rules of the Code of Obligations, the contractor formally reports the defect of the supplied material to demand the replacement of pallets or organise a return to the factory.

If the client nevertheless demands installation despite the written report, the practitioner must record the order in writing, releasing themselves from technical liability regarding subsequent joint openings. Only an exchange of goods with a batch conforming to future climatic requirements guarantees a stable floor after commissioning.

Frequently asked questions

How to resolve divergent results between a capacitance moisture meter and a pin-type device?

The capacitance moisture meter is used solely for rapid non-destructive location but remains sensitive to wood density and surface finishes. In the event of a dispute, resistance measurement with insulated pins driven to one-third of the board thickness is authoritative on site. For definitive legal expertise, only the destructive method of weighing before and after oven-drying according to standard SIA 253 formally settles the disagreement.

Why must the moisture content of a parquet board be measured even before opening the packs?

Original heat-sealed packaging protects the parquet from hygrometric variations during transport and temporary storage. Opening the packs immediately exposes the wood to the building's environment. To verify whether the manufacturer has delivered a product compliant with the correct equilibrium moisture content, measurement must be carried out as soon as a test package is opened, taking the board from the core of the stack to avoid external influences.

What moisture content should be targeted for solid parquet laid on a floor with underfloor heating?

For underfloor heating in Western Switzerland, indoor humidity regularly drops below 35% relative humidity during sustained heating periods. The equilibrium moisture content of the wood is then between 6% and 8%. Wood delivered above 9% will undergo severe shrinkage during the first temperature activation. Standard SIA 253 governs these values to prevent the appearance of major visual or structural defects.

What to do if the delivered batch has a moisture content below 6%?

Excessively dry wood presents the opposite risk: it will absorb ambient moisture as soon as winter ends and swell. This causes destructive lateral thrust, board lifting, or crushing of peripheral expansion joints. Pallets must be quarantined, site management notified, and the supplier required to deliver material stabilised within the hygrometric equilibrium range defined by standard SIA 253.

Texts and standards cited

  • SIA 253Requirements relating to the installation and hygrometric conditions of wooden floor coverings