Key takeaways
- The starting grit is chosen according to board lippage and the thickness of old finishes.
- Each abrasive pass must erase the grooves cut by the preceding grit without skipping any.
- The application of a finish mercilessly accentuates residual micro-scratches under grazing light.
- Standard SIA 253 prescribes a flat and uniform surface condition before any finishing treatment.
Determine the starting grit and comply with the grit size progression
Sanding solid or engineered wood flooring allows no compromise on the chronology of abrasives. The first pass, or starting grit, aims to plane the floor, eliminate lippage between boards, and strip old layers of wear or oxidation. A frequent temptation on the construction site is to start directly with a medium grit to save time or to preserve the thickness of the noble wood. This approach prematurely clogs the abrasive belts, heats up residual resins, and leads to uneven surfacing that violates the requirements of standard SIA 253.
| Initial condition of the wood floor | Starting grit | Intermediate sequence | Finishing grit |
|---|---|---|---|
| Marked deformation, lippage > 1 mm, thick old finish | Grit 24 or 36 | Grit 40, then 60, then 80 | Grit 100 or 120 |
| New unfinished installed wood floor, minor installation lippage | Grit 40 or 50 | Grit 60, then 80 | Grit 100 or 120 |
| Light renovation, superficially worn finish, flat floor | Grit 60 | Grit 80 | Grit 100 or 120 |
The progression between steps relies on a strict mechanical principle: the sole mission of each abrasive is to eradicate the scratches left by the previous pass by progressively reducing their depth. Professional rules prohibit any gap greater than one standard grit jump in the FEPA standardized scale. Going from grit 36 to grit 80 without interposing grit 50 or 60 constitutes a major technical fault. Even if the wood visually appears whitened and clean, the valleys gouged by grit 36 remain open along the grain of the wood.
Understand the mechanism of masked scratches revealed by the finish
The naked eye does not easily perceive micro-crevices on vacuumed raw wood, because fine dust and diffuse light refraction mask surface defects. This optical illusion misleads hurried workers. As soon as the wet phase occurs—whether it is a primer, an impregnating oil, or a water-based sealer—the liquid components penetrate the fibres by capillary action. The liquid causes an immediate raising of the abraded fibres and alters the refractive index of the substrate.
- Initial gouging by roughingCoarse grit (grit 24 to 40) shears the wood fibre deeply and leaves angular furrows visible from an oblique angle.
- Deceptive masking by grit skippingThe direct use of a fine grit (grit 80 or 100) clips the top edges but does not reach the bottom of the furrows, which are temporarily filled with sanding dust.
- Wetting during applicationThe binder of the finish infiltrates the unplaned furrows, saturates the wood unevenly and causes the sheared fibres to swell.
- Definite revelation under grazing lightUpon drying, the varnish or oil tightens the surface film; the roughing hollows appear in the form of arcs of circles or dark stripes, requiring complete rework.
Inspection of the work must imperatively be carried out before opening the containers of finish. The foreman and the team carry out a visual inspection using a grazing light projected parallel to the floor, with the machine stopped and careful dust removal completed. A light test-moistening with denatured alcohol or cleaning spirit allows immediate anticipation of the final refraction on critical areas, notably at edge connections and in doorways.
Execution of intermediate passes and cutting trajectories
On a renovation or new installation construction site, the starting grit does not aim to polish, but to plane the floor. Depending on the initial condition of the wood floor—presence of an old polyurethane sealer, pronounced lippage between solid boards, or warping of old elements—the attack is carried out with an abrasive grit P24 or P36 for severe cases, or P40 for new unfinished work without major flatness defects. This roughing pass deeply cuts into the material: it eliminates excess thickness and creates a geometrically flat surface, but leaves a dense network of microscopic furrows in the wood.
Standard SIA 253 governs wood floor coverings and sets surface condition requirements for delivered work. To comply with these requirements, the sole mechanical function of each intermediate pass is to level the crests and erase the furrows left by the previous grit, replacing them with a narrower and shallower scratch. Wanting to go directly from grit P36 to grit P80 to save time is a fatal method error. Grit P80 cuts the surface crest, but its fine grains cannot reach the bottom of the valleys created by P36. The bottoms of the cuts remain intact, temporarily filled with sanding dust.
| Initial condition of the wood floor | Starting grit | Intermediate grits | Machine finishing grit | Fine sanding / Mesh screen |
|---|---|---|---|---|
| Heavy renovation (paint, glue, major lippage) | P24 or P36 | P50 then P80 | P100 or P120 | Mesh screen P120 to P150 |
| Standard renovation (worn finish, slight deformations) | P40 | P60 then P80 | P100 or P120 | Mesh screen P120 to P150 |
| New unfinished solid wood floor (nailed or glued installation) | P50 or P60 | P80 | P100 or P120 | Mesh screen P120 to P150 |
The trajectory of the passes determines the effectiveness of this progression. Roughing is generally carried out at a 45-degree angle to the direction of the boards to level the edges and correct cupping without gouging the soft grain. The first intermediate pass reduces this angle to 20 or 30 degrees, cutting diagonally across the previous furrow to eliminate it visually and mechanically. Finally, the fine intermediate pass and finishing are carried out strictly in the direction of the wood grain, parallel to the boards, so that the final micro-scratches blend with the natural grain of the timber species.
Surface finishes, perimeter connections and revelation of defects
Work at the perimeters requires discipline identical to that carried out in the open field. The connection between the belt sander and the rotary edge sander represents the most sensitive area. The edges must imperatively follow the same grit sequence as the rest of the room. Using grit P40 with the belt sander then attempting to even out the edges with grit P80 using the edge sander generates an immediate texture disparity. Furthermore, the rotation of the edge sander creates circular scratches that cut perpendicularly across the wood grain; these circular traces must be carefully reduced by regular semi-circular movements, then erased during the pass of the orbital sander or oscillating edge sander equipped with grit P100 or P120.
The ultimate pass before surface treatment uses a heavy single-disc machine or a multi-disc sander equipped with a drive pad and an abrasive mesh screen P120 or P150. This multi-directional pass breaks the last raised fibrils and unifies the surface texture between the centre of the room and the edged perimeters. This step also makes it possible to smooth the wood filler applied after grit P80 for filling joints and cracks.
To validate flatness and the absence of drum marks or orphaned scratches, the wood flooring installer performs an inspection under grazing light before any finish application. The appearance criteria of standard SIA 253 penalize abrasive marks visible in normal daylight at eye level. The contractor thus ensures compliance of the work without risking a claim during the final acceptance of the floors.
Rework protocol after revelation of scratches under finish
When the application of a first coat of primer, sealer or oil highlights circular scratches or longitudinal claws due to a grit skip, no partial or localized surfacing can make up for the work. Standard SIA 253 requires visual regularity of appearance and a homogeneous surface condition without perceptible abrasion marks under grazing light. Attempting to mask a stripe by overloading with varnish or by locally fine-sanding with a fine abrasive creates refraction halos and geometric hollows that accentuate the defect.
- Complete stripping of the film or oilCompletely strip the surface of the room down to the raw wood using the belt sander by choosing the intermediate grit that precedes the observed skip, most often grit 60 or 80, oriented in the axis of the grain or at a 15-degree angle.
- Resumption of the continuous grit sequenceSequentially carry out grit 80 without any omission to erase the coarse pass traces, then grit 100, and finish with grit 120. Connect the edges with the edge sander while strictly observing the same gradation on the perimeters of the wood floor.
- Inspection under grazing light and surfacing with the single-disc machineSweep the room in dim light with a 2000-lumen grazing spotlight oriented perpendicularly to the direction of the boards. Pass a grit 120 abrasive mesh screen on a single-disc machine to unify the textures between edges and centre before re-applying the finishing system.
The cost of complete rework for a 30 m² room is often between 40 and 60 francs per square metre in unrecoverable working time and lost consumables. Strict compliance with the initial grit sizing remains the only technical and economic guarantee on site.
Frequently asked questions
Can you go directly from grit 40 to grit 80 to save time?
No. Grit 40 leaves deep furrows in the solid wood or engineered top layer. Grit 80 does not have sufficient removal capacity to level the crests and erase the bottom of these valleys. If you skip grit 60, the initial claws remain, masked by the sanding dust, and then brutally reappear in the form of dark lines as soon as the oil or sealer wets the fibre.
Why are sanding scratches especially visible near windows?
Natural grazing light coming from glazed bays accentuates the optical contrast between the crests and the furrows of the wood. When the bottom of a scratch not eliminated by the intermediate grit receives the finish, the product accumulates there or alters light refraction. Standard SIA 253 also provides for the assessment of surfaces under intended lighting, which makes these defects immediately contestable during the acceptance of the work.
How to choose the first grit on a heavily soiled oak wood floor?
The initial condition dictates the starting grit: on a thick sealed finish or deformed boards showing significant lippage, start with grit 36 or even 24 to strip without overheating the binder. If the wood floor is newly installed unfinished or simply waxed, grit 40 or 50 is more than enough. A starting grit that is too fine immediately clogs the abrasive and glazes the wood instead of cutting it cleanly.
Must the same grit sequence be used with the edge sander as with the belt sander?
Absolutely. The perimeter of the room must receive exactly the same succession of grits as the central zone treated with the drum. If you sand the centre up to grit 120 but stop the edge sander at grit 80, the difference in the opening of the wood pores will create a flagrant shade boundary around the entire perimeter as soon as a stain, oil or matte sealer is applied.
Texts and standards cited
- SIA 253Wood floor coverings and parquet flooring: requirements relating to substrates, installation, flatness and surface finishes.