Skip to content
Website
🧱 CFC 283Substrate, preparation and underlaysChapter 1 of 10 in the section

Flatness: tolerance for parquet flooring, straightedge measurement and mandatory smoothing compound

This chapter provides the method for the geometric inspection of the subfloor prior to parquet installation. You will learn how to check the deflection under the straightedge in accordance with SIA 253, identify bumps that cause creaking or interlocking failures, and then record your findings to trigger a priced supplementary smoothing operation with the site management.

Key takeaways

  • Standard SIA 253 limits the permissible unevenness under the straightedge to protect the joints.
  • A local bump creates a pivoting point causing persistent creaking and board delamination.
  • Inspection is systematically carried out using a rigid straightedge combined with a set of graduated shims.
  • Any defect found requires a formal notice and the pricing of supplementary remedial smoothing.

Requirements of standard SIA 253 and the physics of parquet creaking

In a wooden floor covering work, the flatness of the subfloor directly governs the mechanical stability of the joints. Standard SIA 253 defines the strict criteria that a screed or raised floor must meet to receive parquet flooring, whether fully glued or installed as a floating floor. If the slab has depressions, the board sags under foot traffic. However, the most destructive technical problem remains the presence of a ridge or a local bump on the mineral subfloor.

When a floating parquet floor rests on a bump imperceptible to the naked eye, this prominence turns into a rigid support point. Each step creates a rocking movement: the element sinks on one side, lifts on the other, and stresses the tongue-and-groove machining or mechanical click locks. This continuous friction between two wood or fibre walls produces an unpleasant squeaking sound. In the medium term, the repetition of this bending shears the machined profiles, creating irreversible height differences between boards and causing edge joints to open.

In glued installation, a bump prevents the uniform crushing of the glue beads applied with a notched trowel. The adjacent areas are left without direct contact with the subfloor, generating hollow-sounding areas underfoot and risks of delamination during seasonal dimensional variations of the wood. The flatness tolerance is therefore not merely an aesthetic requirement, but a guarantee of structural durability for the installer.

Straightedge measurement method and qualification of supplementary smoothing

Checking flatness is the responsibility of the parquet installer during the visual and mechanical inspection of the subfloor before work on the construction site begins. This check is never carried out by eye or using a short level. It requires a systematic procedure over the entire surface to be fitted, particularly along partitions, around floor duct penetrations and at casting joint transitions.

  1. Sweeping and thorough vacuumingThe subfloor must be cleared of all residual laitance, plaster debris or paint splatter. The slightest impurity would distort the seating of the straightedge.
  2. Placement of the 2 m aluminium straightedgeThe rigid straightedge is placed flat on the floor, moved in a fan shape and crossed orthogonally and then diagonally to cover the main circulation areas.
  3. Probing using the calibrated shimThe gap between the bottom of the straightedge and the top of the screed is measured using a bevelled shim or millimetric thickness gauges. The shim must never be forced through.
  4. Marking and locating defectsHigh points to be planed or sanded are circled with wax crayon or red forestry chalk; depressions requiring material addition are hatched with the measured thickness noted.
Diagnosis of deviations and corrective measures according to standard SIA 253
Measurement under a 2 m straightedgeNature of the defect observedConsequence on parquet flooringRequired action
Less than 2 mmConforming to standardStable seating, direct installationValidation of subfloor for installation
Local bump of 3 mmSpot high pointRocking, creaking, joint failureNotice of defect, localized sanding or planing
Depression of 3 to 6 mmContinuous hollow or subsidenceParquet sagging, adhesive voidSupplementary self-levelling smoothing compound over primer
Deviation greater than 6 mmMajor non-conformity of structural workMassive delamination, plane failureWritten notification, refusal to install, screed remediation

Under no circumstances should the parquet installer autonomously correct a non-compliant screed without a written order from the site management. If the subfloor exceeds the tolerances of standard SIA 253, the professional must immediately draw up a written notice stating the precise measurements per room and the risk of damage associated with friction noises. In accordance with the principles of standard SIA 118 and the Code of Obligations governing service contracts, the responsibility for delivering a flat screed lies with the screed trade. However, on construction sites, the client very frequently entrusts the remediation to the parquet installer in the form of supplementary smoothing priced as modification work.

When the smoothing intervention is ordered from the parquet installer, it must be rigorously priced. Provision must be made for the application of a bonding primer compatible with the nature of the screed (cement or calcium sulphate), the pouring of a fibre-reinforced self-levelling smoothing compound suited to the target thickness, as well as the mandatory drying time before resuming wood installation. For a common average smoothing thickness between 3 mm and 5 mm, the cost magnitude generally ranges between 25 and 45 CHF per square metre supplied and installed, including subfloor preparation but excluding prior heavy sanding.

Mapping of bumps and diagnosis of friction noises

On a screed reputed to be ready to receive parquet, flatness defects rarely manifest as regular hollows. They are almost systematically residual bumps, trowel ridges or edge risers that generate the most severe defects. Under a floating parquet floor, a localized ridge creates a mechanical pivot point. During repeated passage by occupants, the board is subjected to permanent cantilever stress. The resilient underlay quickly crushes directly beneath the ridge, and the tongue-and-groove or click-system assembly profiles work under shear stress. This wood-on-wood or wood-on-polymer friction produces the characteristic dry creaking sound often wrongly attributed to the wood material itself, whereas it results from an out-of-tolerance subfloor.

Methodical diagnosis of the subfloor cannot be improvised by eye. The site manager or lead installer moves a 2-metre rigid metal straightedge in a regular grid across the entire surface of the room, both lengthways, crossways and diagonally. Deflection is evaluated using a set of bevelled shims or calibrated thickness gauges slid beneath the aluminium profile. When the straightedge rocks by oscillating around a central point, the bump is immediately located. The parquet installer then draws a clear circle in wax crayon around the anomaly and notes the value of the cantilever effect observed at the ends of the straightedge. A 3-millimetre shim must never pass under a 2-metre straightedge according to the standard requirements of standard SIA 253 governing glued and floating floor coverings.

Remediation protocols and financial compensation for smoothing

When the joint inspection record reveals tolerance exceedances, the parquet installer cannot proceed with installation without engaging their own technical liability regarding future creaking and height differences. The screed delivered by the floor-laying or screed company falls under structural work or heavy finishing work services. Two technical scenarios then apply to correct the support plane before implementing the underlay or full-surface gluing.

Typology of flatness defects and required corrective actions
Nature of the defect observedDeviation measured with straightedgeRecommended remediation methodPotential acoustic impact
Point bump or trowel ridge> 2 mm over 2 m or > 1 mm over 20 cmHeavy diamond-disc grinding with industrial dust extractionWood-on-wood friction and sharp mechanical creaking
Edge subsidence or general depression> 3 mm over 2 mApplication of a bonding primer then self-levelling mortarPumping effect under foot traffic and disengaging clips
Repeated screed undulation> 4 mm over 2 mComplete self-levelling smoothing of at least 3 mm thicknessFull-surface glue detachment or assembly failure

If the subfloor features only isolated bumps, the quickest solution consists of locally planing or sanding the cement or anhydrite using a floor grinder equipped with a diamond disc and connected to a HEPA vacuum cleaner. On the other hand, if the screed exhibits generalized hollows or discontinuous deflections, carrying out supplementary self-levelling smoothing becomes essential. This levelling work must be the subject of a written addendum detailing surface preparation, dust removal, the application of a bonding resin compatible with the future parquet adhesive-sealant, and the average thickness of mortar required.

From a financial and organizational perspective, compensating for a screed defect attributable to a third party requires rigorous pricing transmitted to the site management prior to any intervention. Remedial self-levelling smoothing work is generally priced on the basis of supply and installation including initial keying of the subfloor, meticulous vacuuming, application of the bonding primer and pouring of a fibre-reinforced or self-levelling levelling compound of at least 3 millimetres thickness. Actual costs observed on Swiss French-speaking construction sites are in the order of 25 to 45 CHF per square metre depending on room configuration and the thickness of the compensatory mortar required, an amount to be validated by site order or modification order by the client before starting installation.

Management of flatness disputes and recourse in the event of sagging

When a residual bump is overlooked before clipping a floating floor, the parquet loses its continuous flat support on the screed. The boards are then in a cantilever position, turning the area into a permanent mechanical pivot. With each user passing over it, dynamic deflection causes repeated friction between edge profiles, generating persistent acoustic creaking. In the short term, this abnormal stress leads to the irremediable shearing of the clipped tongues and grooves. Standard SIA 253 imposes a rigorous flatness requirement precisely to prevent these structural defects that ordinary structural work tolerances do not cover.

When inspection with the two-metre aluminium straightedge and bevelled shim reveals non-compliant deflection, the parquet installer has the professional obligation to immediately stop work in the defective area. Remediation of the subfloor defaults to the screed trade. If the execution schedule does not allow for the screed contractor to return, the site management regularly commissions the floor installer to carry out supplementary equalization smoothing. This task is not part of the fixed installation price: it must be quoted and form the subject of a signed purchase order before any mixing takes place. Installing without a written order on a deformed subfloor exposes the professional to bearing full responsibility for subsequent acoustic and mechanical degradation.

  1. Joint inspection record: precise location of high points using the straightedge and chalk marking in the presence of the site management.
  2. Formal notification: written reporting of subfloor non-conformities invoking the rules of good workmanship of the Code of Obligations.
  3. Preparation of the quote: prompt transmission of pricing for ridge sanding or self-levelling equalization smoothing.
  4. Written execution order: mandatory waiting for the signed addendum before applying any primer or laying any board.

Frequently asked questions

What is the flatness tolerance permitted by standard SIA 253 for a floating parquet floor?

For the floating installation of parquet, standard SIA 253 prescribes a maximum deflection tolerance of 3 mm under a 2-metre rigid straightedge placed on the floor. If measurement with the graduated shim reveals a gap greater than this value, the subfloor is considered non-compliant. This strict limit prevents boards from rocking and damaging their joints during repeated pedestrian traffic.

How to properly carry out inspection using the straightedge and bevelled shim?

Inspection is carried out by placing a 2 m straight metal straightedge on the screed, moving it in all directions. A calibrated or bevelled inspection shim is then slid under the straightedge wherever a hollow appears, as well as on bump ridges. The survey must be documented with photos and precise floor plan locations to provide irrefutable technical evidence to the site management prior to intervention.

Why must supplementary smoothing be the subject of a priced addendum?

The parquet installer's initial contract provides for installation on a subfloor deemed compliant with flatness standards. Any remediation of hollows or reduction of bumps implies additional supplies, such as primer and self-levelling mortar, as well as unforeseen labour. The prior establishment of a supplementary quote or site order prevents any subsequent refusal of payment by the client by formalizing agreement on the actual cost of remediation.

Who bears the financial burden when the screed exhibits flatness defects?

The provision of a flat surface within tolerances is owed by the appointed screed company. If the site management commissions the parquet installer to carry out equalization using a self-levelling smoothing compound to avoid a construction site standstill, these additional costs are charged to the structural work trade or deducted from the retention of the failing screed contractor. The parquet installer invoices their services directly to the site management according to the amounts agreed by addendum.

Texts and standards cited

  • norme SIA 253Requirements relating to subfloor flatness and glued or floating floor coverings
  • code des obligationsDuty of care and notification of subfloor defects in the service contract

In the same section