Key takeaways
- Detecting existing reinforcement governs the precise setting-out layout for future drill holes.
- All structural bonding requires dowels that hold a specific technical approval for cracked concrete.
- Cleaning the drill hole directly determines the final bond of the injected resin.
- Tensile tests on sacrificial dowels validate the actual load-bearing capacity of the host element.
Testing old concrete and selecting an anchor for cracked concrete zones
Connecting a new foundation slab, suspended slab or wall to an old structure requires checking the substrate quality before finalising the design. On a construction site, the internal condition of the existing load-bearing element often holds surprises: poor compactness, honeycombing, or highly variable concrete cover. The contractor undertaking the works first examines the site constraints in accordance with art. 3 OTConst, in order to plan operations while limiting the risk of accidents or technical defects. Work systematically begins with a non-destructive detection phase.
- Electromagnetic rebar detectionScan the interface area using a ferromagnetic cover meter or structural radar to locate the longitudinal bars and stirrups precisely. Mark the reinforcement on the wall with a wax crayon to set out drill holes away from conflict zones.
- Visual and acoustic check of compactnessScabble local renders or laitance and sound the concrete with a bricklayer's hammer. A hollow sound indicates delamination or carbonated and crumbling concrete, prohibiting any direct bonding without prior removal back to the sound core.
- Pilot assessment drill holesDrill small-diameter pilot holes to check the drilling resistance felt at the machine, the colour and dryness of the drilling dust, and the absence of internal voids or through-cracks.
In a structural extension connection, the interface zone is systematically considered to be subject to tension or stress redistribution. Consequently, the use of mechanical anchor systems or chemical bonding with a valid European approval for cracked concrete (Option 1) is mandatory. Products intended for uncracked concrete (Option 7) are strictly excluded: they lose their load-bearing capacity as soon as micro-movement or a shrinkage crack appears at the interface between the two concretes.
- Bonded dowel for cracked concrete
- Metal anchor rod or high-bond rebar set with reactive resin (vinylester or pure epoxy), tested and certified according to a European Technical Assessment to transfer shear and tensile forces in a substrate exhibiting standardised crack widths.
Installing dowels, checking by tensile testing and managing tolerances
The performance of a chemical anchor strictly depends on the drilling method and the removal of drill dust. Drill using a rotary hammer drill or diamond coring rig according to manufacturer requirements. Using a wet core drill requires additional cleaning of the internal wall by vigorous brushing to remove the slurry film that prevents resin adhesion. Dust is cleared using oil-free compressed air, alternating with mechanical brushing using a wire brush of suitable diameter, following the standard cycle: blow, brush, blow.
| Setting-out parameter | Permissible tolerance | Consequence on new reinforcement |
|---|---|---|
| Setting-out axis deviation | ± 10 mm | Adjustment of added reinforcement ties |
| Effective drilling depth | - 0 mm / + 20 mm | Guarantee of anchor capacity without risk of punching through |
| Drilling angularity | ± 3° from normal | Need for bevelled washers under baseplates if mechanical dowel |
| Minimum edge distance | Per technical data sheet (min. 5 d) | Risk of concrete spalling due to cone breakout |
To validate the match between the selected product and the actual compactness of the old substrate, carrying out an on-site pull-out test constitutes accepted good practice. Two approaches exist depending on the protocol defined by the civil engineer: the non-destructive proof test on structural dowels, loaded up to a specified service tensile value, or the destructive test carried out to failure on sacrificial dowels installed under identical geometric conditions.
- Installation of hollow-ram tension cylinderPosition the hydraulic cylinder on a distribution stool to prevent the reaction supports from exerting compressive stress on the theoretical breakout cone of the tested dowel.
- Progressive load applicationIncrease pressure in constant increments using a hand pump fitted with a calibrated gauge, recording displacement using a dial gauge.
- Verification of acceptance criterionHold the specified proof load for the required observation time. The absence of measurable slip validates system adhesion for the batch of dowels concerned.
Drilling strategy and preservation of existing reinforcement
Setting out bonded dowels in an existing load-bearing element requires strict coordination between the geometry of the new structure and the existing reinforcement grid. Drilling without prior rebar detection exposes the structure to the cutting of main steel bars, reducing local load-bearing capacity and compromising overall stability under service loads.
- Non-destructive rebar detectionScan the interface area using an electromagnetic cover meter or structural radar to plot load-bearing rebars and stirrups. Mark the bar centres with wax crayon and transfer actual spacings to the setting-out template.
- Adjustment of drill hole locationsShift the drilling centres if a geometric conflict arises with a main rebar. This offset must remain within the limits tolerated by the civil engineer to prevent stress concentrations at the construction joint.
- Mechanical drilling and handling of obstaclesProceed with hammer drilling using a mechanical depth stop. In the event of an immediate strike against an unforeseen rebar, stop the machine without forcing, fill the blind hole with non-shrink mortar, and establish a new centreline according to the approved layout.
Execution control, traceability chain and alignment tolerances
Effective transmission of shear and tension across the joint depends on the perpendicularity of the dowels and the homogeneity of the bonding material. Under art. 364 CO, the contractor performs the work under their personal supervision and procures the means and tools required to guarantee the technical conformity of structural connections.
| Geometric parameter | Workshop / construction site tolerance | Consequence of exceeding tolerance | Corrective measure |
|---|---|---|---|
| Horizontal alignment deviation | ± 5 mm | Torsional force in the new slab | Slotted hole on free sleeve side if specified |
| Dowel spacing deviation | ± 10 mm | Poor shear force redistribution | Recalculation of the anchor group by the engineer |
| Squareness defect (perpendicularity) | ± 2° (approx. ~3 mm over 100 mm) | Expansion joint locking and concrete spalling | Re-bending prohibited; replace with new dowel |
| Effective embedment depth | - 0 mm / + 15 mm | Insufficient pull-out capacity | Deeper drilling after verifying element thickness |
For the protection of workers exposed to mineral dust and chemical splashes during horizontal drilling and resin injection, LAA requires the employer to take all necessary preventive measures that experience has demonstrated and that the state of technology allows. On-tool dust extraction at the hammer drill and wearing sealed safety goggles are therefore essential at the workstation.
Managing bonding non-conformities and engineering arbitration
On a refurbishment construction site, discovering deteriorated structural concrete or dowel slippage during a tensile test requires a targeted stoppage of work. If pull-out resistance fails to reach the proof load prescribed by the design, the foreman must not attempt to retighten or re-inject the rod without technical instructions. The hole is logged as non-compliant on the setting-out drawing.
- Recording and notificationRecord the exact position of the failed anchor, photograph the extraction state or any cracks that appeared in the substrate concrete, and submit the notice to the civil engineering consultancy.
- Structural arbitrationThe engineer evaluates the possibility of drilling an adjacent replacement dowel, respecting the centre-to-centre and edge distances defined by the technical assessment of the resin or mechanical dowel.
- Remediating abandoned holesFill the abandoned hole with a non-shrink bonding mortar to restore confinement and corrosion protection for the existing internal reinforcement.
According to CO, if the material supplied by the client or the ground designated by the client is found to be defective, or if any other circumstance compromises the correct or timely performance of the work, the contractor shall immediately inform the client. The heterogeneity of old concrete typically constitutes such an unforeseen circumstance requiring written instruction from the site management.
The report of the tensile tests, recording the loads achieved without residual deformation for each tested element, is countersigned by the responsible engineer prior to granting any concrete pour approval for the construction joint.
Frequently asked questions
How should you react if the drill bit strikes an existing rebar?
Drilling must be stopped immediately so as not to cut the load-bearing rebar. The core drill or rotary hammer is withdrawn. The blind hole must be cleaned and filled with non-shrink grout. The civil engineer then defines a new offset drilling location, taking into account minimum centre-to-centre distances and the anchor breakout cone in the old concrete.
What protocol must be followed if a tensile test reveals anchor slip?
The dowel is declared non-compliant and decommissioned. The foreman records the incident in the site journal. The cause is investigated: presence of inadmissible moisture, incomplete brushing and blow-cleaning, or inadequate resin curing. The engineer specifies an additional replacement dowel and may require double the testing rate for the batch.
Can chemical resin be heated to accelerate curing in winter?
No. Artificial heating using a blowtorch or heat gun degrades the molecular structure of the bonding mortar and destroys its mechanical properties. A resin formulation approved for low temperatures must be selected, cartridges must be stored in warm conditions prior to extrusion, and the full curing time stated on the technical data sheet must be strictly observed before applying load.
What angular tolerance is acceptable when drilling for shear dowels?
The drilling axis must remain perpendicular to the interface plane, with a maximum angular deviation not exceeding 2 to 3 degrees. Excessive inclination alters the load-bearing axis of the dowel, concentrates abnormal stresses on the edges of the existing concrete, and prevents proper alignment of rebar boxes or couplers in the adjacent new structure.
Texts and standards cited
- COmaterial and ground: the contractor is liable for the sound quality of the material supplied; if the material supplied by the client or the ground designated by the client is found to be defective, or if any other circumstance compromises the correct or timely performance of the work, the contractor shall immediately inform the client, on pain of bearing the consequences (para. 3)