🧱 CFC 211.1Pathologies of reinforced concrete, diagnosis and strengtheningChapter 10 of 10 in the section

Protecting a concrete surface: water repellent, anti-carbonation and maintenance

Faced with sound reinforced concrete that is exposed to weathering or de-icing salts, applying surface protection prevents premature deterioration of the reinforcement. This chapter guides you in distinguishing the actual role of impregnations from film-forming coatings, setting application criteria, and recording renewal cycles intended for the structure's maintenance plan.

Key takeaways

  • A water repellent blocks liquid water without preventing carbon dioxide from penetrating into the concrete.
  • An anti-carbonation coating forms a continuous film that slows gas diffusion and neutralises moisture.
  • Standard SIA 269 requires the monitoring and predictable degradation of surface treatments to be incorporated.
  • Refurbishment cycles must be communicated to the client as early as the planning phase.

Distinguishing the action of a water repellent from that of an anti-carbonation coating

Intervening on a sound structure requires a functional analysis of the specified product. Too often on a construction site, the terms impregnation, water repellent, and anti-carbonation paint are confused, leading to serious durability errors. A surface water repellent — generally silane- or siloxane-based — penetrates into the capillary pores of the concrete without creating a surface film. By modifying the surface tension of the cementitious matrix, it repels water in liquid form as well as dissolved chlorides, while leaving the substrate completely open to water vapour diffusion. Conversely, a surface water repellent presents virtually no barrier to the diffusion of gaseous carbon dioxide.

Integral waterproofer
Admixture incorporated into the mix during concrete batching to reduce overall capillary absorption, distinct from hydrophobic impregnation applied to a hardened surface.

In contrast, an anti-carbonation coating consists of a film-forming system, based on pure acrylic resins or copolymers in water-borne or solvent-borne phases. Its formulation aims for a very high specific resistance to carbon dioxide diffusion, quantified by an equivalent air layer thickness. It stops the drop in the potential of hydrogen of the concrete around passivated rebars, while forming a continuous barrier against driving rain. However, this coating requires a substrate perfectly prepared by light grit-blasting or high-pressure washing to ensure mechanical adhesion without blistering.

Technical comparison of surface protection systems
CharacteristicSurface water repellent (silane)Anti-carbonation coating (film-forming)
Mechanism of actionHydrophobic impregnation of poresFormation of a continuous surface film
CO2 penetrationUninhibited (free diffusion)Impermeable barrier to gas diffusion
Water vapour diffusionTotal (breathable substrate)Moderate to permeable depending on formulation
Visual appearance of the facingUnchanged (no visible film)Opaque, satin or tinted matt appearance

Defining maintenance intervals and recording the maintenance plan according to standard SIA 269

Managing the life cycle of a structure relies on the series of standards for maintaining the value of structures, particularly standard SIA 269. Upon acceptance of protection works on a sound structure, the contractor does not hand over an eternal barrier. Environmental aggressions such as freeze-thaw cycles, ultraviolet radiation, and abrasion progressively degrade the effectiveness of the active molecules or cause chalking of the film-forming resins. The structure documentation file must compulsorily state the inspection and re-application deadlines required to preserve the structure.

  • Annual visual inspection for fouling, incipient cracking, and debonded areas.
  • Water absorption test using a Karsten tube every 3 to 5 years on water-repellent concrete.
  • Direct pull-off adhesion testing and examination of chalking every 5 years on film-forming coatings.
  • Systematic recording of the intervention history in the structure's maintenance logbook.

For a surface hydrophobic impregnation with a high active content (liquid monomer silane or cream), functional durability is usually between ten and fifteen years depending on exposure to sea spray or driving rain. Beyond this period, surface tension decreases and the beading effect disappears. For anti-carbonation coatings, renewal of the topcoat must be planned every twelve to fifteen years, provided the intermediate film remains sound. These time horizons determine the calculation of the overall life-cycle cost that the client must anticipate financially.

Application criteria on sound concrete: hydrophobic impregnation versus film-forming system

On an existing reinforced concrete structure determined to be sound during the condition survey according to standard SIA 269, the choice of surface treatment aims to block external aggressive agents before any reinforcement degradation occurs. The distinction between a surface hydrophobic impregnation and a film-forming anti-carbonation coating rests on the physics of fluid transport within the surface pore network.

Technical comparison of surface protection systems for sound concrete
Technical characteristicHydrophobic impregnation (silane / siloxane)Anti-carbonation coating (acrylic / polyurethane)
Main actionModification of pore surface tension without mechanical blockageCreation of a continuous film impermeable to gases and liquids
Substrate penetration2 to 6 mm depending on porosity and active contentPurely mechanical and chemical surface adhesion
Barrier to carbonation (CO2)Zero to very low: permeable to atmospheric gasesHigh: diffusion resistance equivalent to several metres of air
Water vapour permeabilityExcellent: the concrete matrix continues to dry freelyMedium to low: risk of blistering in the event of residual moisture
Performance across cracksIneffective: bridges no active or dormant cracks greater than 0.1 mmCrack-bridging capacity varies depending on the elasticity of the selected resin
Required substrate preparationHigh-pressure cleaning, removal of release agentsLight grit-blasting or shot-blasting, dust removal, bonding primer

An integral waterproofer, incorporated during mixing at the time of pouring, differs fundamentally from a surface water repellent. It alters the entire concrete volume by reducing overall capillary absorption, but does not compensate for curing defects or early cracking. When intervening on an existing structure within the framework of standard SIA 269, only surface hydrophobic impregnation applied by low-pressure sprayer or roller makes it possible to waterproof the facings without altering the raw appearance of the material.

Acceptance protocols on the construction site and planning of maintenance cycles

The effectiveness of a surface protection system depends directly on inspection during execution on the construction site. For a hydrophobic impregnation, the site foreman checks the penetration depth by taking chips or cores and spraying coloured water onto the fresh cross-section. For an anti-carbonation coating, measurements cover dry film thickness (micrometres) and direct pull-off adhesion.

The service life communicated to the client must be formulated rigorously. No surface treatment is permanent. Degradation results from freeze-thaw cycles, ultraviolet radiation, and mechanical wear. The maintenance plan established according to standard SIA 269 specifies the timeframes for visual inspections and renewal operations to prevent the carbonation front from reaching the reinforcement.

  • Surface hydrophobic impregnation: inspection of the beading effect every 3 to 5 years by means of a Karsten tube test; full reapplication recommended every 10 to 12 years depending on weather exposure.
  • Anti-carbonation coating: visual inspection of defects (chalking, blistering, crack initiation) every 2 to 3 years; refurbishment of the topcoat every 12 to 15 years, provided primer adhesion is maintained.
  • Pre-existing integral waterproofer: monitoring of the carbonation profile by core drilling and phenolphthalein testing every 10 years on elements exposed to salt spray or run-off water.

At a contractual level, the site foreman ensures that the condition of the substrate provided by the client permits product application in accordance with the manufacturer's technical datasheets. If surface compactness is compromised by overly aggressive grit-blasting or carbonation that is already too deep, the contractor notifies the client in accordance with art. 365 CO in order to determine the preparatory measures required before applying the protection.

Managing protection failures and contractor obligations

On a sound reinforced concrete structure, the occurrence of coating blistering, premature chalking, or a loss of the beading effect signals a breach in the protective barrier. Water and carbon dioxide then resume their advance towards the passivated reinforcement. The contractor must respond from the first visual observations to arrest the degradation kinetics before the carbonation front reaches the reinforcement.

  1. Diagnosis of adhesion and carbonation depthPerform direct pull-off tests (dolly pull-off) to quantify the adhesion of the failing system. Take cores or make a cut to spray phenolphthalein and measure the thickness of concrete already neutralised relative to the remaining cover.
  2. Mechanical removal of the deteriorated systemComplete stripping of the film-forming coat or the saturated surface layer by dry grit-blasting, low-pressure hydro-blasting, or mechanical shot-blasting, without damaging the integrity of sound laitance or fracturing the aggregates of the facing concrete.
  3. Reapplication and traceability in the maintenance planApply a new system complying with adhesion and CO2 diffusion requirements on the decontaminated substrate. Update the structure documentation file in accordance with standard SIA 269 to recalculate the date for the next maintenance intervention.

In accordance with art. 365 CO, the contractor is liable for the sound quality of the material they provide. If the treatment products delivered by the supplier present an intrinsic adhesion defect or if the concrete characteristics jeopardise the proper application of the protection system, the contractor informs the client.

Frequently asked questions

How can one differentiate the effect of a surface water repellent from an integral waterproofer?

An integral waterproofer is incorporated during batching to modify the capillary porosity of the entire cementitious matrix. A surface water repellent is applied by impregnation onto the hardened facing; it lines the pores without filling the voids, creating hydrophobicity that repels liquid water while allowing the concrete to breathe. It primarily protects against the penetration of dissolved aggressive agents without altering the internal structure of the underlying reinforced concrete.

Does a water repellent block the carbonation of reinforced concrete?

No. A surface water repellent modifies the surface tension of the pores to prevent liquid water from penetrating, but it does not constitute a physical, gas-tight obstacle. Atmospheric carbon dioxide passes through the hydrophobic pores and continues the cement neutralisation process in the presence of residual moisture. To block CO2, applying a certified anti-carbonation paint or film-forming coating remains technically indispensable.

What maintenance interval should be planned according to standard SIA 269?

According to standard SIA 269 for the maintenance of structures, a visual inspection of external facings is carried out every 2 to 5 years to detect blistering, crazing, or staining. For a silane-siloxane hydrophobic impregnation, renewal generally occurs between 8 and 12 years depending on climate exposure. A film-forming anti-carbonation coating requires refurbishment of the topcoat or full renewal every 12 to 15 years.

Why does an anti-carbonation coating debond prematurely?

Debonding often results from botchy substrate preparation: presence of residual laitance, unremoved formwork release oil, or excessive moisture content during application. If water vapour contained within the structure cannot escape through a product whose permeability value is incorrectly calibrated, internal pressures cause blisters under solar radiation or frost action, destroying the mechanical bond of the protective system.

Texts and standards cited

  • norme SIA 269Basis for maintenance, examination, and intervention on existing load-bearing structures
  • CO art. 365Material and site: the contractor is liable for the sound quality of the material they supply; if the material supplied by the client or the site designated by the client is found to be defective, or if any other circumstance compromises the proper or punctual execution of the work, they shall immediately inform the client, on pain of bearing the consequences (para. 3)

In the same section