Key takeaways
- Prior micrometric monitoring confirms whether crack opening is stabilized or still subject to movement.
- Epoxy resin restores structural monolithism, whereas flexible polyurethane ensures deformable waterproofing.
- Injector spacing strictly corresponds to half the thickness or the total thickness of the member.
- Destructive coring of at least fifty millimetres verifies the actual filling rate of the binder.
Determine crack movement and select the resin family
Treating a discontinuity in reinforced concrete strictly begins with analysing its mechanical behaviour over time. A stabilized crack undergoes no further variations in opening under the effects of residual hydraulic shrinkage or seasonal thermal cycles. Conversely, an active crack continues to move under operational loads or thermal gradients. Injecting a rigid resin into a live crack inevitably leads to the formation of a new parallel fracture in the adjacent sound concrete, as tensile stress is not dissipated.
| Crack condition | Intended objective | Type of binder | Mechanical behaviour |
|---|---|---|---|
| Stabilized (dormant) | Restore load transfer | Low-viscosity epoxy resin | High adhesion, rigid and monolithic bond |
| Active (live) | Ensure water tightness | Flexible polyurethane resin | High elastic elongation without load transfer |
| Damp under pressure | Immediately stop water ingress | Expanding polyurethane foam | Preliminary rapid expansion, followed by a resin |
To rebond a structural element whose static design requires continuity of compressive and tensile stresses, fluid epoxy is the only acceptable binder. Its very low viscosity allows it to saturate openings as narrow as two-tenths of a millimetre. When the crack acts as a waterproofing relief on an underground structure subject to free deformations, elastomeric polyurethane is selected: it accommodates repeated dimensional variations without debonding from the concrete edges.
Set out injectors, carry out keying, and inspect by coring
Setting out injectors, whether surface-mounted or screwed into inclined boreholes crossing the crack, follows rigorous geometric rules. For high-pressure screw-in injectors, drill holes are made at forty-five degrees to the concrete face, alternating on either side of the crack path, to intercept the fracture plane in the middle of the cover zone. Spacing along the crack line is aligned with the wall thickness: a pitch equal to half the thickness of the member is generally adopted, never exceeding its total thickness.
- Surface sealing of the pathOpen a slight chamfer if necessary, then seal the crack surface using a thixotropic epoxy mastic to prevent lateral leakage of the fluid under pressure.
- Purging and air blowingRemove dust from boreholes and the crack path using dry, oil-free compressed air to ensure polymer adhesion to the mineral substrates.
- Progressive upward injectionInject the resin from the lowest point of the structure. As soon as pure, air-free product emerges from the upper injector, cap off the current point and move the pumping nozzle upward.
Conformity inspection cannot be limited to monitoring resin consumption on the pump pressure gauge. Technical acceptance of a structural reinforcement requires taking a concrete core sample across the plane of the crack. This core, with a minimum diameter of fifty millimetres, is drilled at a representative distance from an injector. The engineer examines the core sample to verify that the crack filling rate reaches at least ninety per cent of the effective depth and that failure during a subsequent tensile test occurs in the sound concrete and not at the polymer interface.
Kinematic behaviour and choosing between rigid and flexible resin
On a reinforced concrete structure, injecting without having characterised the activity status of a fissure invariably leads to secondary structural defects. An active crack continues to undergo opening variations due to daily or seasonal thermal gradients, differential foundation settlements, or fluctuating live loads. Conversely, a stabilized crack has exhausted its initial cause, such as early plastic shrinkage, a temporary formwork-stripping phase, or hydraulic shrinkage following complete drying of the structural work. Preliminary inspection using vernier calliper gauges or optical crack monitors fixed across the edges provides data on this behaviour over a representative cycle.
- Stabilized crack versus active crack
- A stabilized crack exhibits a fixed opening that undergoes no further measurable variation under service loads. An active crack undergoes cyclic or progressive deformations; any rigid restraint of its edges would transfer tensile stresses, causing a new fracture in the immediate vicinity.
| Crack characteristic | Recommended resin family | Targeted mechanical function | Effect of a specification error |
|---|---|---|---|
| Stabilized, stress transferred (shrinkage complete) | Solvent-free pure epoxy (high bond strength) | Rigid structural rebonding, restoration of monolithism | Underdosing or flexible product: failure to transfer shear stresses |
| Active, thermal or mechanical variations | Elastic polyurethane or flexible acrylic resin | Ductile void waterproofing without kinematic restraint | Rigid epoxy injection: new parallel crack in adjacent sound concrete |
| Active pressurised water ingress | Temporary water-reactive expanding polyurethane foam | Emergency stoppage of water ingress prior to final bonding | Complete washout of epoxy resin before curing |
Structural bonding requires a two-component epoxy resin of very low viscosity, capable of penetrating into cracks smaller than 0.2 mm by capillary action. This polymer cures with negligible shrinkage and develops a tensile strength exceeding that of the concrete itself (routinely exceeding 30 N/mm²). However, its elongation at break remains minimal, generally confined below 2 to 3%. Applying this material to an active crack edge therefore turns the treated area into an undeformable hard spot: the induced tensile stress exceeds the tensile strength of the concrete and generates a parallel secondary crack a few centimetres from the injected line.
Injector spacing, keying, and validation by coring
Setting out injectors (or packers) governs the complete filling of the void without trapped air pockets. For mechanical packers with expandable sleeves inserted into 45° boreholes intersecting the crack plane, the fundamental rule requires spacing strictly proportional to the thickness of the structural element or the presumed depth of the discontinuity.
- Surface sealing and injector installationThe crack surface is sealed using a thixotropic epoxy mastic to contain injection pressure. Injectors are drilled staggered on either side of the crack to intersect the plane at mid-thickness of the wall, or surface-bonded if drilling risks cutting tensioned reinforcement located by electromagnetic scanning.
- Executing keying under controlled pressureInjection progresses from the lowest point to the highest point on a vertical wall, or from one end to the other on a slab. The product is pumped at moderate pressure (often between 2 and 15 bar depending on the opening) until pure resin, free of air bubbles, bleeds out of the adjacent open packer. The latter is then closed and the operation proceeds sequentially.
- Destructive inspection by through-coringAfter full curing (at least seven days at 20 °C), a 50 to 100 mm diameter core is extracted perpendicular to the crack plane. The core undergoes direct visual examination to measure the effective filling rate and an indirect (Brazilian) or direct tensile test. Failure must imperatively occur in the sound concrete and not within the epoxy bonding plane.
Coring remains the definitive method of investigation when demonstrating to site management that the mechanical continuity of the element has been restored. A continuous filling rate exceeding 90% of the cracked depth is generally required to validate structural rebonding. If the contractor observes continuous residual voids during drilling or an adhesion failure indicative of unblown drilling dust, a high-pressure reinjection procedure or an adjustment of technical provisions is required. Pursuant to art. 365 CO, if an unforeseen circumstance or unexpected behaviour of the substrate jeopardises the stability of the structure, the contractor notifies the client.
Management of injection non-conformities and remediation after failed coring
On a structural strengthening site, injecting a through-crack does not on its own guarantee the restoration of monolithism. If the inspection coring report shows insufficient filling, loss of bond, or premature refusal of injection, site management and the foreman must determine the structural status of the works without delay.
- Presence of continuous residual voids over more than one-third of the thickness inspected in the test core.
- Failure of epoxy resin to set, generally caused by incorrect component proportioning or concrete temperature below technical datasheet requirements.
- Debonding of resin at concrete edges, indicating excessive moisture or insufficient cleaning of boreholes with dry compressed air.
- Reappearance of adjacent cracks after curing, reflecting an error in kinematic diagnosis between active and stabilized cracks.
If the substrate designated by the client exhibits unexpected kinematic behaviour or if water ingress compromises the adhesion of the rigid epoxy resin, the contractor exercises the duty to notify. Pursuant to art. 365 CO, the contractor is liable for the good quality of the material supplied; if the material supplied by the client or the ground designated by them is found to be defective, or if any other circumstance jeopardises the regular or punctual execution of the work, the contractor informs the client.
- Immediate backfilling of the test coreThe cylinder cored for investigation weakens the reinforced concrete section. It must be reconstituted using a non-shrink grout or micro-concrete cast behind watertight formwork following application of a bonding slurry.
- Drilling a second line of offset packersTo remediate an unsaturated section, install a new set of injectors at 45 degrees staggered relative to the initial points, intersecting the fracture plane upstream of the identified defect.
- Switching to an adapted pressurised injectionIf residual moisture is detected in the internal void, substitute the rigid structural epoxy with temporary hydrophilic polyurethane pre-keying, followed by a moisture-tolerant epoxy resin approved by the civil engineer.
Frequently asked questions
What should be done if the test core shows crack filling of less than 80%?
The civil engineer from site management must assess the residual load-bearing capacity of the section. If the required monolithism is not achieved, the element cannot be approved for tensile load transfer. The contractor must then drill new inclined packers, intersect the unsaturated crack plane, and perform reinjection with fluid epoxy resin at stabilised low pressure, then backfill the core hole with micro-concrete.
How should an inspection core hole in a reinforced concrete wall be properly backfilled?
The core hole locally weakens the watertight or load-bearing wall. Thoroughly clean the cavity by blowing with compressed air, apply a bonding agent around the cylindrical circumference, then pack the void completely using a high-performance non-shrink grout. The surface must be floated flush with the existing concrete face to ensure visual continuity and corrosion protection for surrounding reinforcement.
Why can a crack bonded with rigid epoxy resin crack again right next to it?
Cured rigid epoxy resin has a higher tensile strength than the cementitious concrete matrix. If the initial crack was not fully stabilized and was still subject to thermal variations or structural differential settlements, mechanical stresses are instantly transferred to the adjacent unreinforced concrete zone. This phenomenon confirms an initial diagnostic error: the situation required a flexible polyurethane resin.
What protective equipment is mandatory for plant operators during high-pressure injection?
Pressurised injection presents a severe chemical splash hazard in the event of packer failure or hose burst. Operators must wear sealed safety goggles or a full face shield, thick nitrile gloves resistant to solvents and reactive resins, and protective overalls. Safety helmets remain mandatory in accordance with site operational regulations to prevent impacts and falling tools.
Texts and standards cited
- CO art. 365materials and ground: the contractor is liable for the good quality of the material supplied; if the material supplied by the client or the ground designated by them is found to be defective, or if any other circumstance jeopardises the regular or punctual execution of the work, the contractor shall immediately inform the client, failing which they shall bear the consequences (para. 3).