Skip to content
Website
🧱 CFC 211.1Pathologies of reinforced concrete, diagnosis and strengtheningChapter 4 of 10 in the section

Structural or surface crack: distinguish them before raising alarm

Faced with cracking in reinforced concrete, the construction site team must make an objective initial diagnosis without panicking. This chapter teaches you to characterise the crack path, measure crack width according to SIA 262 requirements, analyse the exact location relative to supports and unequivocally identify the threshold justifying work stoppage or intervention by the civil engineer.

Key takeaways

  • Superficial plastic shrinkage cracking does not compromise the load-bearing capacity of the structure.
  • Allowable crack widths are strictly regulated according to the exposure class defined in standard SIA 262.
  • A diagonal 45-degree orientation near a support signals a major shear force risk.
  • Any active or through-crack requires the installation of gauges and the intervention of the civil engineer.

Characterise the geometry and location of the crack on the load-bearing element

On a reinforced concrete structure, cracking is a normal mechanical phenomenon linked to the behaviour of the material under tension. The practical challenge on site consists of distinguishing between a cosmetic surface defect with no static consequence and a warning sign of local failure. To achieve this, the site foreman primarily observes the orientation of the crack path and its exact geometric position relative to lines of support, columns or beams.

Typology of surface and structurally induced cracks
Crack typeTypical locationDominant orientationProbable mechanical cause
Crazing or plastic shrinkageSurface exposed to wind, upper faces of slabsRandom, hexagonal or disordered networkSurface tension during early evaporation
Simple bendingSoffit of slab or beam at mid-spanPerpendicular to the span axis (vertical or transverse)Exceedance of the tensile strength of unreinforced concrete
Shear forceWeb of beam or slab, in the immediate vicinity of supportsInclined at approximately 45 degrees towards the supportExcessive shear, insufficient shear reinforcement stirrups
Differential settlementShear walls, raft-to-wall junctionsContinuous diagonal cutting across storeysFoundation movement or settlement of a support point

A surface crack never goes through the element. It generally stops before the first layers of steel reinforcement. Conversely, a through-crack visible on both faces of a wall or between the soffit and top surface of a slab proves that the full cross-section is subjected to tensile stresses not accommodated by the design reinforcement.

Measure crack width according to SIA 262 and set the alert threshold

Evaluating the severity of a crack relies on accurately measuring its width, carried out using an optical crack microscope or a crack width gauge graduated to tenths of a millimetre. The use of imprecise tools distorts the diagnosis and can trigger unjustified alerts or, conversely, conceal a risk of accelerated corrosion of non-prestressed reinforcement.

The limiting value of crack width calculated under quasi-permanent load combinations aims to ensure the durability of the structure and the visual appearance, depending on the exposure class and the sensitivity of the reinforcement.

norme SIA 262

In standard practice for an office or residential building, allowable nominal crack width thresholds w_nom generally vary between 0.2 mm and 0.4 mm. A width below 0.2 mm in a dry indoor environment in no way jeopardises the durability of the reinforcement and falls within the serviceability limit state. As soon as the width exceeds 0.3 mm in a damp environment or one exposed to chlorides, the steel is no longer durably protected by the alkalinity of the concrete.

  1. Initial measurement and markingClean the area without scraping the crack line. Measure the maximum width using an optical crack microscope. Note the date, time and ambient temperature directly on the concrete next to the measuring station.
  2. Kinematic monitoring using crack monitorsInstall a millimetric crack monitor or a measuring disc to check whether the crack is dormant or active. A crack whose width changes within a few days signals a critical redistribution of internal forces.
  3. Notification to the site managementDraft a formal notice accompanied by a dimensioned sketch indicating length, orientation, distance to supports and measured width.

When the measurement exceeds 0.5 mm on a primary load-bearing element, the foreman suspends the application of new imposed loads and immediately calls upon the civil engineering consultancy. Likewise, if the crack exhibits out-of-plane stepping—that is, a level offset between both lips of the crack discernible to the touch—the kinematic behaviour of the member is compromised. Pursuant to art. 365 CO, the contractor immediately informs the client whenever a circumstance jeopardises the proper or timely execution of the structure, an imperative procedure as soon as overall stability is at stake.

Mechanical interpretation based on trajectory and loading

Distinguishing a superficial defect from structural damage requires direct reading of the fracture lines on the reinforced concrete element. A crack is never random: its path traces the principal tensile trajectories that the unreinforced concrete was unable to resist. The site manager must compare the visual survey with the static scheme of the structure before considering precautionary measures.

Typology of defects on load-bearing members and associated mechanism
Zone of the elementOrientation of the crack pathUnderlying mechanismStructural classification
Bottom face of slab or beam within the spanPerpendicular to the span axis (vertical)Simple bending due to exceedance of tensile strengthNormal structural (stabilised under service load if reinforced)
Immediate vicinity of supports (walls, columns)Inclined at approximately 45 degrees towards the supportShear force or initiation of punching shearCritical structural (risk of brittle failure without warning)
Top face directly over a continuous supportTransverse to the span axisNegative bending moment over support (tension in upper zone)Common structural (to be monitored with respect to corrosion)
Column shaft or compressed shear wallParallel to the compressive force (vertical)Bursting due to insufficient confinement or crushingMajor structural (load-bearing capacity compromised)
Free surface of a freshly poured slabRandom network, multidirectional orientationPlastic shrinkage or early superficial dryingSurface defect (no impact on overall stability)

The orientation relative to the reinforcing steel bars provides a decisive clue. A straight crack following the main reinforcement layer exactly indicates plastic settlement of fresh concrete beneath the bars or the onset of carbonation-induced corrosion with swelling of the rebar. Conversely, a through-crack cutting across the bars at right angles reflects tensioning of the member under external load.

Monitoring protocols and thresholds for summoning the civil engineer

Not every abnormal opening requires an immediate shutdown of operations, but it does mandate rigorous traceability. On the construction site, the management team must record crack path development using strain gauges or dated plaster tell-tales. The objective is to determine whether the phenomenon is passive (stabilised after shrinkage or initial loading) or active (progressive opening under live loads or differential settlement).

  1. Marking and loggingTrace the ends of the crack path on the surface using indelible marker, noting the survey date and the width measured with the optical crack microscope.
  2. Installation of crack monitorsInstall millimetric vernier gauges or strain measuring targets on either side of the crack lips in the areas of greatest opening.
  3. Monitoring load cyclesRecord width variations during the application of heavy construction site loads (storage of masonry packs, transit of machinery, striking of props).
  4. Formal technical alertTransmit the photographic dossier and numerical records to the site management and the engineering consultancy as soon as critical criteria are exceeded.

On-site intervention by the civil engineer becomes mandatory when the defect compromises structural safety or durability under SIA 262. The site foreman alerts the site management without delay if the width exceeds the nominal allowable value of the element, if the crack traverses the entire thickness of the concrete (loss of watertightness or failure of crossing reinforcement) or if signs of localized crushing appear in the compression zone. The contractor strictly observes their duty to inform under the Code of Obligations (CO) whenever an unforeseen circumstance threatens the stability of the entrusted works.

Crisis protocol and emergency measures in case of critical cracking

The sudden appearance of an oblique crack in the immediate vicinity of a support or the abrupt opening of a crack within the span signals local failure of the reinforced concrete member. Faced with active kinematics, the construction site team must neutralise the risks without waiting for the conclusions of an in-depth static calculation.

  1. Securing the area and load reductionImmediately bar access to the area below and above using rigid barriers. Remove imposed construction site loads present on the slab or deck: pallets of bricks, concrete skips or handling equipment.
  2. Installation of emergency proppingPlace shoring towers or heavy-duty props beneath the threatened member, without attempting to force jacking to close the gap. Contact must relieve bending or shear without introducing uncalculated parasitic counter-stresses.
  3. Technical survey and formal summonsInstall strain gauges or micrometric tell-tales across the crack path. Transmit to the civil engineer a detailed report including macro photographs, crack width measured with a graduated gauge and exact position relative to load-bearing members.

The contractor who identifies a defect jeopardising the stability of the works must alert the site management. Pursuant to art. 365 CO, if any circumstance compromises the proper or timely execution of the works, the contractor informs the client. The civil engineer remains the only party authorised to determine structural strengthening solutions: installation of bonded composite plates on the slab soffit, controlled jacking, supplementary post-tensioning or reinforced concrete jacketing.

Frequently asked questions

Does a plastic shrinkage microcrack require intervention by the civil engineer?

No. Crazing or random superficial shrinkage cracks of limited depth less than 0.2 mm wide do not affect the load-bearing capacity of the structural work. These defects stem from drying physics and surface effects. If the opening remains stable within the tolerances of standard SIA 262 and does not reach the non-prestressed reinforcement, the static integrity of the load-bearing member is not compromised.

Why does a 45° oblique crack near a column demand immediate propping?

A crack oriented at 45° at supports indicates an exceedance of shear resistance or an imminent risk of punching shear. This type of failure in reinforced concrete is brittle and sudden, unlike simple bending which provides warning through deflection. Immediately relieving the zone with load-bearing props prevents the abrupt collapse of the slab-column connection.

How can one distinguish a normal bending crack from a major structural defect?

In zones of maximum bending moment, fine vertical cracks below the limits of standard SIA 262 are anticipated to mobilise the tension steel. Conversely, if the crack penetrates through the entire thickness of the reinforced concrete, exceeds 0.4 mm or propagates towards the upper compression zone, the reinforcement may be yielding, which requires verification by the engineer.

Which measuring instrument should be prioritised on the construction site before the engineering office arrives?

A transparent crack comparison gauge enables an immediate direct visual assessment of crack widths. To track changes over time, install without delay a mechanical dial-gauge vernier crack monitor screwed on either side of the crack lip. This provides reliable records in tenths of a millimetre to support emergency decisions by the site management.

Texts and standards cited

  • SIA 262Standard for concrete structures: structural design and durability requirements
  • CO art. 365Materials and ground; mandatory notice if a circumstance compromises the proper execution of the works