🧱 CFC 211.1Pathologies of reinforced concrete, diagnosis and strengtheningChapter 6 of 10 in the section

Strengthening with bonded carbon laminate: substrate preparation and bonding

Structural strengthening using carbon-fibre-reinforced polymer composite laminates increases the load-bearing capacity of slabs and beams without adding dead weight to the existing structure. After this chapter, you will know how to prepare the substrate to the required tolerances, apply the epoxy adhesive without air voids, and integrate the thermal protection essential to prevent fire-induced failure.

Key takeaways

  • The strength of the strengthening system depends entirely on mechanical adhesion to the prepared concrete.
  • The epoxy adhesive loses its structural stiffness as soon as the temperature exceeds its glass transition temperature.
  • Flatness checks under a straightedge prevent premature fibre pull-out caused by peeling.
  • Fire protection must insulate the resin to ensure the required structural stability in a fire event.

Mechanical preparation and flatness tolerances under standard SIA 269

The application of externally bonded carbon fibre reinforced polymers (CFRP) falls within the maintenance of existing load-bearing structures governed by standard SIA 269. This method aims to resist additional bending moments or tensile forces without altering the clear headroom or overloading the supports. However, the composite only develops its nominal strength if the transmission of shear stresses at the concrete-adhesive interface is ensured. Substrate cleaning tolerates no laitance, formwork release oil, or paint.

End peeling (peeling)
Brittle failure through pull-out of the concrete cover occurring at the end of a bonded composite laminate, caused by high concentrations of normal and shear stresses.

Surface treatment is carried out by sandblasting, closed-circuit shot blasting, or diamond disc grinding. Aggressive chiselling or bush-hammering is prohibited because it creates internal microcracks in the surface matrix of the concrete. Pore opening must be complete and aggregates exposed over at least fifty percent of the application area. The surface cohesion of the treated concrete must be verified on site by direct pull-off testing before any bonding takes place.

Preliminary concrete substrate checks prior to bonding
Checked parameterMeasurement methodMinimum technical requirement
Surface tensile strengthBonded metal dolly with dynamometerMinimum mean value according to engineer's specification
Flatness under a two-metre straightedgeAluminium straightedge and thickness gaugeDeflection below system supplier tolerances
Substrate moistureCapacitive measurement or calcium carbide methodDry surface, moisture content compatible with epoxy

To eliminate this risk, hollows are levelled using an epoxy mortar compatible with the bonding resin, while ridges are ground down flush with a grinder equipped with a dust extraction hood. Final dust removal is performed immediately before installation using an industrial vacuum cleaner with a HEPA filter; simple sweeping or the use of non-deoiled compressed air is strictly prohibited. Air quality at the workstation must remain compliant with the general provisions of the construction work ordinance.

Application of structural adhesive and thermal risk management

The structural adhesive is a two-component thixotropic system based on epoxy resin. Mixing of the two components is carried out at low speed using a helical paddle until a uniform colour without marbling is achieved. The quantity prepared must strictly correspond to the practical pot life, which drops rapidly as the ambient temperature rises. Application cannot take place if the substrate temperature is less than three degrees above the dew point.

  1. Laminate preparationClean the bonding face of the composite with a specific volatile degreaser to remove any mould release residue or workshop dust.
  2. Rooftop-profile adhesive applicationApply the adhesive to the laminate in a crowned bead that is thicker in the centre, ensuring the paste is forced towards the edges during roll-pressing.
  3. Roll-pressing with a rigid rollerPress the carbon plate from the centre towards the ends using a hard rubber roller to expel entrapped air.
  4. Joint thickness inspectionCheck for a continuous, uniform bead extruded on each side of the laminate and scrape off the excess with an angled spatula.

The civil engineer responsible for structural safety often highlights a major limitation: polymer resin has a relatively low glass transition temperature, often between forty-five and sixty-five degrees Celsius. Beyond this value, the organic matrix softens and the adhesive's modulus of elasticity collapses. Load transfer between the concrete and the laminate then ceases abruptly, causing premature failure of the strengthening system well before the intrinsic limits of the carbon are reached.

If the engineer's calculations demonstrate that the bare, unheated load-bearing structure withstands the accidental fire load case without the composite, the thermal protection may be dimensioned solely to prevent spalling. Otherwise, where strengthening is required to carry permanent and quasi-permanent loads in a fire situation, the insulation assembly forms an integral part of the externally bonded reinforcement system. Any damage to this protective barrier must be notified in accordance with art. 365 CO in order to avoid the execution of work compromised by a lack of coordination.

Adhesion testing and substrate acceptance before roll-pressing

The effectiveness of structural strengthening with carbon composite laminates depends exclusively on shear stress transfer at the interface between the epoxy resin and the cementitious matrix. Standard SIA 269 governs work on existing structures and requires verification of substrate suitability prior to any final application. Even with a decontaminated, dedusted, and geometrically corrected surface, a lack of internal cohesion in the underlying concrete renders bonding entirely ineffective. The site manager or site foreman must ensure that the direct tensile strength of the prepared concrete is formally validated by on-site pull-off tests.

Direct tensile pull-off tests involve core-drilling the prepared concrete to a depth of 15 to 20 mm, bonding a rigid metal dolly of standardised diameter, and applying a perpendicular tensile force until failure. The failure mode is decisive: failure must occur 100% within the concrete itself, proving that the surface strength exceeds the stresses transferred by the composite. If failure occurs at a lower value or reveals surface delamination due to internal cracking, the area must be rejected. Under art. 365 CO, the contractor notifies the client if the material or ground provided compromises the proper execution of the work, which includes the inability of an existing substrate to carry the intended loads.

Concrete substrate acceptance criteria for composite laminate strengthening
Monitored parameterOn-site measurement methodConformity criterionRequired corrective action
Surface cohesionDirect pull-off test (steel dolly)Mean >= 1.5 N/mm² (minimum isolated value >= 1.0 N/mm²)Additional mechanical removal or structural reprofiling
Residual moistureCapacitive moisture meter or carbide methodMoisture content < 4% (per resin technical data sheet)Forced drying by ventilation or indirect radiant heating
Substrate temperatureInfrared contact thermometer>= 3 °C above ambient dew pointPostponement of roll-pressing or controlled heated enclosure
Cleanliness and dustStandardised tape pull-off testAbsence of visible traces of cement dustIndustrial vacuuming with high-efficiency HEPA filter

Thermal vulnerability and fire protection installation

The primary advantage of carbon strengthening lies in providing high load-bearing capacity without significantly increasing the weight of structures. However, the polymer matrix and structural adhesive represent the absolute weak point of this system in the event of a fire. While carbon fibres withstand extreme temperatures without failure, the epoxy resin reaches its glass transition temperature (Tg) at just 50 °C to 65 °C. Once this threshold is exceeded, the adhesive transitions from a rigid glassy state to a soft rubbery state, instantly losing its modulus of elasticity and shear load transfer capacity.

When the civil engineer dimensions the strengthening under standard SIA 269, two design situations must be distinguished: the standard ultimate limit state and the accidental fire situation. If the structural element does not possess sufficient internal reinforcement to support permanent loads and a portion of variable loads during thermal failure of the laminate, passive fire protection becomes mandatory. This requirement is governed by the fire protection regulations of the Association of Cantonal Fire Insurers (VKF/AEAI), which specify the required resistance (often EI 60, EI 90, or REI 120 depending on building use).

  1. Drying and complete curing of the epoxy adhesiveWait until the final Shore hardness of the bonded system is reached before any mechanical intervention or application of thermal insulation cladding, i.e. at least 3 to 7 days depending on the construction site temperature.
  2. Application of bonding primer or mechanical spacingSpray a bonding bridge chemically compatible with the resin or install offset stainless steel mechanical hangers to avoid any through-anchorage that would destroy the longitudinal fibres of the strengthening system.
  3. Installation of fire-resisting encasement or mortarInstall an assembly of mineral calcium silicate fire-resisting boards sealed and screwed together without drilling into the laminate, or apply a thick vermiculite-cement spray coating of a thickness determined by the target EI rating.
  4. Inspection of insulation returns at anchor endsAlways cover the anchorage toe of the laminate and extend at least 300 mm beyond the ends of the strengthening system to eliminate lateral thermal bridges.

Management of bonding non-conformities and corrective actions

On a structural strengthening construction site under standard SIA 269, the slightest anomaly observed during application or adhesion testing compromises tensile force transfer. If a flatness defect remains, if delamination is detected by sound, or if the epoxy adhesive begins to gel before roll-pressing, the element loses its function as externally bonded reinforcement.

As soon as a substrate or adhesive non-conformity appears, the site foreman halts work. Under art. 365 CO, the contractor immediately informs the client if the material supplied by the latter or the ground designated by them is found to be defective, or if any other circumstance compromises the proper or timely execution of the work. This written notice protects the contractor and allows the civil engineer to order remedial removal or system reconfiguration.

  1. Detection of delamination or adhesive voidAcoustic hammer testing reveals a hollow sound beneath the cured laminate. If the unbonded area exceeds the threshold defined by the engineer, the laminate must be carefully cut and ground out without nicking the underlying reinforcement bars, then replaced after reprofiling.
  2. Insufficient cohesive failure on pull-off dolliesIf the direct tensile test on a control area fails to reach the contractually required value or exhibits failure in the bond line rather than in sound concrete, the entire batch installed with that mix is rejected for lack of adhesion.
  3. Exceeded open time or unsuitable temperatureTacky resin that no longer extrudes under the pressure roller forms a dry skin preventing wetting of the laminate. All fresh material and composite must be removed immediately, the concrete cleaned with an appropriate solvent, and ground again with an abrasive wheel.
  4. Failure of fire-resisting protectionA poorly fixed insulation shell or board leaves the epoxy adhesive exposed to premature heating. The mechanical fixing of the thermal shield must be rectified without drilling into or stressing the carbon laminate.

Frequently asked questions

How should you react immediately if the resin begins to gel in the pail during application?

The exothermic reaction in the mix is irreversible. As soon as the mixture warms up and loses its fluidity, the pail must be discarded immediately without attempting to spread the product onto the concrete. Applying adhesive that is gelling prevents flattening of the beads and causes massive voids beneath the laminate, inevitably leading to rejection of the work during the engineer's acceptance inspection.

What should be done when a direct tensile test fails within the adhesive body rather than in the concrete?

Cohesive failure within the adhesive indicates improper mixing, surface contamination, exceeded open time, or an excessively cold substrate during application. This premature failure proves that the bond line will not transfer the forces calculated under standard SIA 269. The engineer must be notified in writing; the laminate from the affected batch must be removed and the substrate prepared back to bare concrete.

Is it permitted to patch a local high spot on the concrete just before bonding the laminate?

No, fresh patch repair mortar does not possess the mechanical strength required to withstand structural shear. If a high spot exceeds the flatness tolerance, only mechanical correction by dry diamond grinding with dust extraction is permitted. Any hollows must be filled beforehand using a compatible epoxy mortar that has fully cured prior to roll-pressing.

Can the thermal protection board be fixed directly through the carbon laminate?

Under no circumstances. Any mechanical drilling through the composite severs the unidirectional fibres and destroys the load-bearing capacity of the strengthening reinforcement calculated by the design engineer. The added fire insulation must be bonded to the soffit using an approved thermal adhesive or suspended mechanically using metal anchors set into the reinforced concrete, strictly outside the footprint and width of the laminate.

Texts and standards cited

  • norme SIA 269Basis for maintenance and conformity assessment of existing load-bearing structures
  • CO art. 365materials and ground: the contractor is liable for the sound quality of the materials they supply; if the materials supplied by the client or the ground designated by them is found to be defective, or if any other circumstance compromises the proper or timely execution of the work, they must immediately inform the client, failing which they will bear the consequences (para. 3)