Key takeaways
- Continuous concreting and thorough compaction prevent water paths that are impossible to seal after backfilling.
- The waterstop must remain centred and perfectly straight throughout the entire pour.
- Scabbling the construction joint guarantees perfect adhesion without residual laitance.
- Visual inspection under the groundwater table imperatively precedes the placement of backfill against the walls.
Designing the white tank and installing waterstops
In basement construction, the "white tank" principle relies on the reinforced concrete structure's own ability to ensure watertightness without an external bituminous membrane. According to standard SIA 262, this performance requires a specific mix design limiting porosity, a controlled water/cement ratio, and dense skin reinforcement designed to distribute shrinkage cracking. The required watertightness class specified in the contract defines the tolerance level for internal moisture ingress, ranging from the total absence of seepage for high-grade plant rooms to minor damp patches accepted in underground car parks.
- Waterstop
- Flexible elastomer or thermoplastic profile, positioned in the core or on the surface of the construction joint to block interstitial water.
The recurring weak point of any white tank is located at the interface between the raft foundation and the wall base. A watertight construction joint requires the rigorous installation of a sealing profile or waterstop. The latter must be mechanically fixed every 25 centimetres to specific metal brackets to prevent any tilting or folding under the pressure of fresh concrete. Any joint between sections must imperatively be made by hot-welding with a heating blade; simple overlaps are strictly prohibited as they create an immediate infiltration path under hydrostatic head.
| Profile type | Location | Jointing method | Point of vigilance |
|---|---|---|---|
| Internal ribbed waterstop | At the centre of the wall thickness | Thermal welding with heating blade | Strict centring between reinforcement |
| External ribbed waterstop | At the bottom of the raft formwork | Butt-to-butt thermal welding | Mechanical protection prior to pouring |
| Metal waterstop with coating | At the raft-wall construction joint | Clamping bracket or welding | Continuity of concrete cover |
Executing construction joints, vibrating the mass and signing off before backfilling
Once the raft has been poured, the preparation of the construction joint surface determines the final watertightness of the structure. Before erecting the wall formwork, the team completely removes the cement laitance by mechanical scabbling, high-pressure water jetting or bush-hammering. The final surface must present exposed, rough aggregate. Any residue of dust, formwork release oil, cut tie wires or sawdust is removed using an industrial vacuum cleaner or a compressed-air lance before closing the formwork panels.
- Cleaning and scabbling the construction joint starterScabble the wall bearing zone with a light chipping hammer or by superficial hydro-demolition as soon as the kicker forms are stripped, in order to expose the gravel without damaging the edges of the sealing profile.
- Installation of emergency injection hosesFasten the porous injection hoses in the centre of the joint, against the construction joint, to allow subsequent resin sealing should local porosity appear under hydrostatic loading.
- Concreting in regular layers and compactionPour the wall in 50-centimetre thick lifts. Plunge the poker vibrator vertically into the underlying layer without touching the waterstop or the formwork.
- Visual inspection and sign-off under hydrostatic loadMethodically inspect the interior walls after temporarily shutting down groundwater lowering and before placing the backfill soil.
The contractor must keep in mind that concrete tanking can never be effectively repaired from the inside once the excavation is backfilled. Pursuant to art. 365 CO, the contractor immediately gives notice of any defect in the ground or risk compromising the proper execution of the works. High-pressure injections from the inside remain costly palliatives, often uncertain under continuous hydrostatic pressures. Complete inspection must therefore take place before any soil is placed: the external faces of the walls must be accessible for examination, locally sealed if dampness appears, and the perimeter drainage systems must be approved.
Watertightness requirements according to standard SIA 272 and limits of internal remediation
In Swiss construction, integral reinforced concrete tanking – commonly known as a white tank – derives its watertightness from the density of its cementitious matrix and the geometric detailing of its discontinuities. Structural design is governed by standard SIA 262, whilst the functional watertightness performance of the underground structure is contractually established according to standard SIA 272. Each room use imposes a strict required watertightness class, ranging from the total absence of visible moisture to localized seepage tolerated for unfinished plant rooms.
| Class | Functional requirement | Permissible surface manifestation | Typical basement use |
|---|---|---|---|
| Class 1 | Completely dry | No trace of moisture, no dark spots | Archive rooms, sensitive storage, server rooms |
| Class 2 | Dry | Local damp patches permitted without droplet formation | Plant rooms, residential cellars, laundry rooms |
| Class 3 | Damp | Very localized droplets and seepages tolerated | Underground garages, communal car parks, access ramps |
| Class 4 | Wet | Continuous water drops, temporary water trickles tolerated | Unfinished service tunnels, stormwater retention basins |
To achieve the specified class, controlling early cracking caused by thermal and autogenous/drying shrinkage is essential. In accordance with the design principles of standard SIA 262, the civil engineer defines a minimum reinforcement ratio aimed at limiting theoretical crack widths to values where concrete self-healing remains active under a constant head of water. However, on the construction site, the thickness of the raft foundation and the arrangement of rebars demand flawless placement to guarantee the specified cover.
Control of joints, installation of waterstops and pre-backfill protocol
The most sensitive point of a watertight enclosure remains the geometric interface between the foundation slab and the perimeter vertical elements. The horizontal watertight construction joint must be mechanically prepared by careful scabbling or high-pressure washing to eliminate cement laitance prior to pouring the walls. In this critical zone, the internal mechanical sealing system relies on a continuous waterstop, whose rigid positioning determines the overall durability.
- Securing and fixing the waterstop profileTie the metal or elastomer waterstop to the through reinforcement using dedicated installation brackets. The strip axis must be aligned in the centre of the joint, perfectly vertical, without twisting or kinks. End splices must imperatively be executed by butt thermo-welding to ensure complete continuity of the physical barrier.
- Installation of emergency injection hoses and microperforated ductsFasten the resin injection hoses in close contact with the construction joint, parallel to the waterstop profile. Access ports and junction boxes must be grouped and protected inside the enclosure to enable potential high-pressure resin pumping in case of residual honeycombing.
- Vibration and pouring below the construction joint planePlace an initial bed of bonding mortar or reduce the maximum aggregate size for the first cubic metre of wall. Lower the poker vibrator vertically down to contact with the construction joint without striking the sealing profile, to prevent gravel pockets forming directly under the anchoring ribs.
- Joint formal inspection prior to backfillingFully strike the formwork from the exterior faces of underground walls and wash the surfaces with clean water. Systematically look for areas of segregation, through-cracks or poor compaction. Any patch repair or localized waterproofing treatment on the external face must be executed prior to backfill approval.
Perimeter backfilling must never commence without the site management's formal approval report. Fill materials must be placed in successive compacted layers without damaging any external protective layers or displacing connected drainage installations. A defect left undetected before backfill turns a simple casting imperfection into a complex dispute involving disproportionate remediation costs.
Managing infiltration damage and precautionary measures before backfilling
Observing water ingress on an underground wall dictates an immediate halt to backfilling operations. Once the soil has been backfilled and compacted against the structural work, pinpointing the exact origin of a leak becomes highly uncertain. Water often travels several metres along structural discontinuities before emerging internally. In accordance with art. 365 CO, the contractor immediately gives written notice to the client of any observed anomaly that jeopardizes the integrity of the works or indicates a discrepancy with project requirements.
Diagnosis begins with a precise visual mapping of the defects: through-cracks, concrete segregation at the wall base, or misalignment at the watertight construction joint. If an injection hose was installed as a backup along the waterstop, the team injects it under low pressure using polyurethane resin or acrylic gel, monitoring material progress up to the vent ports. In the absence of an injectable preventive system, 45-degree angle boreholes must be drilled on either side of the defective area to intercept the joint at mid-thickness of the concrete.
- Record the level of the groundwater table or surface water ingress via piezometer before any intervention.
- Install high-pressure injection packers anchored into sound concrete, clear of superficial gravel pockets.
- Log every volume of grout or resin injected as well as refusal pressures for each work run.
- Keep access to external walls unobstructed until the required watertightness class according to good building practice is formally certified.
If concreting exhibits severe defects resulting from poor compaction at the wall foot, external remediation remains the only durable guarantee. In accordance with the requirements of standard SIA 262, damaged or severely porous cover zones are mechanically chipped away by hydrodemolition or scabbling down to the sound core, before rebuilding with shrinkage-compensated mortar and applying a supplementary membrane prior to backfilling.
Frequently asked questions
How should one react immediately upon discovering a gravel pocket when stripping formwork from a watertight wall?
The area must be sound-tested with a hammer to determine the extent of the gravel pocket, and all backfilling must be stopped. The contractor gives notice to the site management in accordance with the duties under the Code of Obligations (CO). Deconsolidated concrete is removed by scabbling until a dense matrix is reached and reinforcement is fully encased. The cavity is then patched with shrinkage-compensated structural mortar compatible with standard SIA 262 before inspection.
Can a watertight construction joint be injected as soon as underground walls are stripped?
No. Injecting a preventive hose system installed against a waterstop is only carried out after the thermal shrinkage of the concrete has stabilized, generally 28 days after pouring. Performing this injection too early exposes the resin bead to mechanical rupture under the effect of residual structural shrinkage. This would compromise achieving the required watertightness class for the basement room.
What should be done if a construction joint injection hose is blocked before use?
Clear water should first be flushed through under pressure to try and clear fresh embedded laitance. If the passage remains completely blocked, angled drilling becomes mandatory. Holes are drilled at a 45-degree angle to intersect the joint plane at the water barrier, allowing metal packers to be installed directly into the defective structural discontinuity.
Why is backfilling the excavation prohibited before flooding or groundwater rise?
As long as the excavation remains open, direct visual inspection allows infiltrations through the raft foundation or walls to be detected and precisely located. After backfilling, the soil conceals the water entry point, making external repairs destructive and extremely costly. Preliminary visual inspection remains the only reliable way to verify that the structure meets watertightness requirements.
Texts and standards cited
- CO art. 365materials and ground: immediate notice to the client in case of defects or circumstances jeopardizing the works
- norme SIA 262Concrete structures: requirements relating to materials, execution and cover tolerances