🧱 CFC 201 / 211.0Mortars, site-mixed concretes and placement productsChapter 7 of 10 in the section

Masonry mortar: strength classes, batching and admixtures on site

This chapter provides professional criteria for selecting the appropriate mortar for the substrate rather than relying on a default mix. You will learn to match the strength class to the properties of the brick or stone, to correctly proportion air-hardening and hydraulic binders, and to manage the actual working life after mixing on your construction sites.

Key takeaways

  • The strength of the mortar must remain lower than or equal to that of the masonry unit being laid.
  • Historic rubble masonry requires a flexible lime mortar to prevent spalling of the faces.
  • Plasticising or air-entraining admixtures improve workability without requiring detrimental excess mixing water.
  • Knocking up mortar that has begun to set permanently destroys its internal crystalline bonds.

Matching the strength class to the mineral substrate

On structural work construction sites, the knee-jerk reaction of using a cement-rich mortar to guarantee strength produces the opposite of the intended effect. An overly rigid mortar concentrates mechanical and thermal stresses instead of distributing them uniformly. When masonry undergoes differential settlement or dimensional variations, cracking runs through the clay bricks or autoclaved aerated concrete blocks rather than dissipating harmlessly within the joint network.

Mortar strength class
Standardised designation identifying the minimum compressive strength at 28 days, expressed in megapascals by the letter M followed by its numerical value (for example M5 for 5 N/mm² or M10 for 10 N/mm²).
Compatibility between mortar class and common substrates according to Swiss Romande practice
Standardised classCompressive strengthRecommended substratesPrescribed binders
M2.52.5 N/mm²Soft rubble stone, molasse sandstone, historic bricksAir lime or natural hydraulic lime NHL 2
M55.0 N/mm²Standard clay units, calcium-silicate bricks, lightweight shuttering blocksCompo mortar with NHL 3.5 lime and CEM II cement
M1010.0 N/mm²High-density clay units, heavy concrete blocks, reinforced masonryPortland-composite cement CEM II/A or B
M2020.0 N/mm²Infrastructure works, massive plinths, walls under heavy loadsHigh-strength cement CEM I or CEM II

Compliance with recognized trade standards requires a deformable interface between rigid prefabricated or natural units. Under art. 365 CO, the contractor is liable for the sound quality of the material he provides and must report defective or unsuitable components. If the specification prescribes a standard mortar incompatible with sensitive historic materials, the bricklayer must take action before installation.

Mastering batching, admixtures and working time

The design of a site-mixed mortar requires consistent discipline regarding the water/binder ratio and the selection of the sand grading curve, ideally a washed 0/4 mm. The introduction of admixtures must address a specific application constraint and must not serve as a remedy for dusty sand or inadequate mixing.

  • Water-reducing plasticisers improve fluidity whilst maintaining the water/binder ratio to guarantee final mechanical strengths.
  • Air-entraining agents create a system of stable microbubbles that increases the deformability of the bedding mortar and enhances resistance to freeze-thaw cycles.
  • Set-retarding admixtures stabilise the paste in mortar tubs during hot summer days or on construction sites located far from the batching plant.
  • Water-resisting admixtures reduce capillarity in the first three base courses exposed to surface water splashing.
  1. Visual check and substrate wettingDust down the units to be laid and moderately moisten porous bricks to prevent them from drying out the fresh mortar through rapid capillary suction.
  2. Consistent batching and mixingAdd the aggregates, binders, then clean water containing the admixture measured with a volumetric dispenser. Mix for three full minutes in a vertical-axis pan mixer or a concrete mixer.
  3. Monitoring of working lifeLay and adjust units within the workability window, generally 90 minutes at 20 °C. Systematically discard any mortar that has started to stiffen in the mix.

Regarding workstation organisation, the application of art. 82 LAA requires preventing accident risks and occupational illnesses by providing protective equipment suitable for handling highly alkaline mineral binders. Bricklayers must wear impermeable gloves and safety goggles when pouring bags of lime and cement into the mixing drum.

Substrate and mortar compatibility: choice of binders and defects resulting from incompatibility

Selecting a laying mortar does not simply mean aiming for the highest mechanical strength. On the construction site, the most common mistake is systematically using a rich cement mortar to lay all types of blocks. An overly rigid and dense mortar on a soft substrate causes major damage. The technical rule demands that the modulus of elasticity and strength of the mortar must always be lower than or equal to those of the assembled material; otherwise, stresses will concentrate within the masonry units rather than in the joints.

Mortar behaviour and compatibility according to the nature of the mineral substrate
Nature of substratePrescribed binderTarget classRisk if mortar is too hard
Soft natural stone (molasse, porous limestone)Pure natural hydraulic lime (NHL 2 or NHL 3.5)M2.5Spalling of edges, vapour entrapment, stone deterioration
Traditional clay units (modular brick, SwissModul)Compo mortar (CEM II cement + NHL lime)M5 to M10Through shrinkage cracking, spalling under thermal stress
Autoclaved aerated concrete or ground insulation blocksDedicated thin-bed adhesive mortarM10Massive thermal bridges, shearing of the interface under thermal expansion
Heavy manufactured concrete blocksCEM II / A or B cement mortarM10 to M15Insufficient bond if the mortar is under-dosed in binder

For the renovation of historic buildings or repairing heritage components, the use of pure cement is prohibited. Lime mortar for old buildings ensures the breathability of the masonry and provides structural flexibility capable of absorbing differential settlement movements. Air lime or natural hydraulic lime ensures consistent moisture exchange, preventing moisture trapping that destroys stones by frost action. A contractor who identifies a deteriorated substrate or one unsuitable for the prescribed mortar must act in accordance with art. 365 CO: if the material supplied by the client or the building ground designated by him is found to be defective, or if any other circumstance jeopardises the regular or punctual completion of the work, he must notify the client.

Rheology, site admixtures and management of working life

Adding admixtures to mortar mixed at the site batching plant or in a concrete mixer profoundly alters its physical properties in both the fresh and hardened states. The two most widely used families are air-entraining agents and water-reducing plasticisers. A plasticiser reduces the water/binder ratio whilst maintaining the workability required for full mortar bedding. An air-entraining agent creates a system of microbubbles that improves frost resistance and helps the trowel glide, but overdosing this product abruptly reduces the strength class.

The working life after mixing constitutes the strict operational limit beyond which the mortar loses its bond performance. When cement setting begins, the hydration process is irreversible. Adding water to the mix to soften a batch that is starting to stiffen is strictly prohibited. This knocking up destroys the emerging crystalline structure, doubles future drying shrinkage, and cuts the final mechanical strength by more than half.

  1. Monitoring working timeMeasure the time elapsed since the introduction of water. In summer temperatures exceeding 25 °C, the working time is reduced to approximately 45 minutes without a retarding admixture.
  2. Protecting the mortar tubCover mortar tubs on the scaffolding with a damp plastic sheet to prevent surface drying caused by wind or direct solar radiation.
  3. Disposal of stiffened remnantsAs soon as lumps appear or trowel workability is lost, the remaining batch must be discharged into the mineral waste skip without any attempt to re-wet it.

Managing mortar non-conformities and setting disputes on the construction site

On a masonry construction site, a mix design error or an exceeded working life quickly results in burnt mortar, delamination under load, or shear cracking. Faced with a mix setting too quickly or a rigid cement mortar mistakenly applied to molasse or historic brick, the site foreman must halt laying immediately. Knocking up mortar that has begun to set with water permanently destroys the formation of calcium silicate hydrates and cuts the final mechanical strength by more than half.

When incompatibility stems from a specification unsuitable for the bedding substrate, art. 365 CO requires the contractor to notify the client if any circumstance jeopardises the regular or punctual completion of the work. This written notice must be submitted prior to assembly to propose substituting an M10 cement mortar with a compo mortar or NHL 3.5 natural hydraulic lime mortar, thereby preventing water vapour blockage and spalling of soft stone.

  1. Identification and halting of the batchIdentify the defect (loss of plasticity, premature desiccation) and record the batch numbers or mixing report in the construction site logbook.
  2. Removal of fresh coursesTake down bricks or rubble units laid with the compromised mix while the mortar has not hardened, then thoroughly clean the mortar beds with a stiff brush.
  3. Formal reportingNotify the site management in accordance with the rules of the Code of Obligations (CO) if the issue arises from aggregates or an incorrect batching instruction.

If the hardened mortar exhibits abnormal friability after seven days, core drills for compressive strength testing must be ordered. Underpinning or deep repointing with lime mortar will remedy the defective area following technical approval by the site management.

Frequently asked questions

Can M10 mortar that is beginning to stiffen in the wheelbarrow be rehydrated?

No. As soon as setting begins, adding water breaks the emerging hydrate crystals without restoring cohesion. This practice produces a washed-out, porous and friable mortar with no mechanical strength. If the working life after mixing has elapsed, the entire batch must be discarded into the mineral waste skip, with no attempt at mechanical or manual re-mixing at the workstation.

Why must factory-made class M10 mortar be prohibited on molasse masonry?

Class M10 mortar has an excessively high modulus of elasticity and very low vapour permeability compared to soft natural stone. Pore water becomes trapped behind the rigid joints. Under the effect of freeze-thaw cycles, mechanical stresses cause the edges of the molasse to spall, with the harder mortar progressively destroying the adjacent bedding stone.

Which admixture should be added for masonry work in hot, dry, windy weather?

A set-retarding admixture combined with a water-reducing plasticiser maintains workability without drowning the mix. The admixture delays the clinker hydration peak without altering the subsequent hardening curve. On the construction site, pre-wetting the bricks and immediately protecting fresh masonry beds with damp tarpaulins remain mandatory to prevent premature desiccation of the mortar.

What is the minimum strength class to aim for regarding an internal load-bearing clay brick wall?

For standard load-bearing clay brick masonry, the required standard mortar class is M5. This compo or factory-made mortar guarantees a compressive strength of 5 N/mm² at twenty-eight days, providing an optimal compromise between structural strength, bond to perforations and sufficient flexibility to absorb minor differential settlements of the structure without through cracking.

Texts and standards cited

  • CO art. 365material and building ground: the contractor is liable for the sound quality of the material he provides; if the material supplied by the client or the building ground designated by him is found to be defective, or if any other circumstance jeopardises the regular or punctual completion of the work, he must immediately notify the client, under penalty of bearing the consequences thereof (para. 3).