Key takeaways
- Breakout removes all degraded or carbonated concrete down to a sound, rough substrate.
- Corroded rebars must be fully cleared around their entire circumference, then brushed and passivated immediately.
- The bonding coat is applied onto a saturated surface-dry substrate, without any bleeding.
- The choice of repair mortar class ensures mechanical compatibility with the structure.
Deep substrate breakout and treating corroded rebars
Durable repair of a spall systematically begins with the total removal of crumbling concrete or concrete contaminated by carbonation. Reprofiling mortar placed on a friable or contaminated substrate will debond under freeze-thaw cycles or mechanical stress. The work is carried out using a light pneumatic chipping hammer (under 5 kg) or a light percussion chisel, so as not to crack the internal matrix of the parent concrete. The edges of the breakout area must be saw-cut or cut square to a minimum depth of 10 to 15 mm to avoid feathered edges, which lead to premature spalling of the repair product.
- Mechanical concrete breakoutClear friable concrete down to refusal on the hard, sound substrate. Remove carbonated concrete beyond rusted bars over a length of at least 50 mm past the visibly sound area.
- Rebar strippingExpose the steels by fine grit blasting, mechanical wire brushing or careful grinding to remove all traces of oxide to bright metal cleanliness.
- Passivator applicationApply immediately by brush a mineral or epoxy-cement passivation slurry or primer over the entire perimeter of the prepared bars, in two cross coats without holidays.
Apply the bonding coat, reprofile with thixotropic mortar, and cure carefully
Reprofiling vertical spalls or the soffits of slabs requires a shrinkage-compensated thixotropic repair mortar capable of resisting gravity sag without formwork. The product is selected according to standard classes (R1 to R4). For load-bearing civil engineering works and building structures subject to high stresses, the site manager will specify a class R3 or R4 mortar characterised by a high modulus of elasticity and excellent compressive strength. For non-structural elements or cosmetic repairs, a class R1 or R2 is sufficient.
| Class | Structural use | Compressive strength | Typical destination |
|---|---|---|---|
| Class R1 | Non-structural | ≥ 10 MPa | Finishing skim, fine cosmetic fairing |
| Class R2 | Non-structural | ≥ 15 MPa | Aesthetic repairs, non-structural balcony edges |
| Class R3 | Structural | ≥ 25 MPa | Columns, shear walls, lintels in standard buildings |
| Class R4 | Structural | ≥ 45 MPa | Civil engineering structures, car parks, slabs under heavy traffic |
Managing substrate moisture is the most critical factor for mechanical bonding. Concrete must be saturated with clean fresh water at least two hours before intervention, then wiped: the surface must be matt and free of any liquid film at the time of contact. On this prepared substrate, a mineral bonding slurry is applied in accordance with system specifications, vigorously brushed into the surface texture. Thixotropic mortar is then applied wet-on-wet, using a trowel or float, in successive passes of 10 to 40 mm, compacting the material firmly to expel trapped air around the rebars.
In the event of a work stoppage on the construction site or doubts regarding residual load-bearing capacity after exposing heavily degraded rebar sections, the contractor notifies the site management in accordance with the duty of care under the Code of Obligations (CO). The unit cost of complete reprofiling including steel treatment typically ranges from 180 to 350 CHF per average repair spot depending on access.
Mortar selection according to destination and compatibility of reprofiling systems
Reprofiling degraded concrete cannot be improvised using standard compo mortar or ordinary cement grout. As soon as repair concerns a load-bearing element or one exposed to weathering (balcony edges, corbels, car park columns), the operative must select a shrinkage-compensated mortar, fibre- or synthetic-resin-reinforced, exhibiting mechanical and elastic characteristics compatible with the parent substrate concrete. Ready-to-use factory-made mortars are categorised into structural or non-structural repair mortars. On a structure subject to service loads, using a structural class mortar is mandatory to ensure compressive stress transfer without perimeter cracking.
| Structural destination | Required mortar class | Target modulus of elasticity | Key mix characteristic |
|---|---|---|---|
| Main load-bearing elements (pillars, beams, slab soffits) | High-performance structural mortar | High (close to substrate concrete) | Shrinkage-compensated, high mechanical bond, pronounced thixotropy |
| Facades, parapets, architectural mouldings without load transfer | Non-structural or fairing mortar | Low to moderate | Fine grain, easy smoothing, aesthetic compatibility |
| Areas exposed to de-icing salts (access ramps, kerbs) | Structural mortar resistant to freeze-thaw cycles | High | Low permeability to water and chloride ions |
Incompatibility of the modulus of elasticity is the primary cause of premature debonding in thick repairs. If the hardened mortar exhibits excessive stiffness compared to the aged substrate, differential thermal stresses shear the interface. Conversely, a material that is overly deformable under load transfers the full load onto neighbouring rebars. The site manager must check the manufacturer's technical data sheet to ensure product compliance with the tender documents and civil engineer requirements.
High-thickness placement protocols, hand compacting, and protection against desiccation
Thixotropic consistency enables mortar to hold on soffits and vertical surfaces without formwork up to single-layer thicknesses governed by product grain size. Whenever a cavity exceeds the permissible sag limit, reprofiling must be built up in multiple successive passes. Each intermediate pass is left rough by scratching with a notched trowel to provide a direct mechanical key for the subsequent pass. No curing agent or film-forming compound may be sprayed between passes, as this would break the mechanical bond.
- Compacting and packing around steelsFirmly press mortar using a trowel or stainless steel float beneath and behind passivated rebars to eliminate air voids or shadowing effects that conceal a lack of material.
- Progressive profiling buildupApply material starting from the back of the cut outward, pressing layers firmly to force out residual air and align the surface flush with the existing face.
- Finishing and surface compactionStrike off the surface with a straightedge or trowel as soon as the mortar starts setting, then float with a damp sponge without adding surface water to avoid washing out the binder.
- Maintaining curing moistureProtect the repair immediately against direct action of wind and sun by applying dampened geotextile kept under plastic sheeting for several consecutive days.
Adherence to trade standards during execution is inseparable from construction site safety. In accordance with art. 82 LAA, the employer takes all necessary measures to prevent occupational accidents and health hazards, notably when mixing very fine, corrosive cementitious powders or using angle grinders for deburring. Regarding overall construction site liability, art. 229 CP notes that intentional or negligent violation of trade standards during construction or demolition work endangering life or bodily integrity exposes offenders to criminal penalties.
Managing non-conformities and remedying defects on the construction site
On a refurbishment construction site, repair failure almost always manifests as a hollow-sounding debonding, early shrinkage cracking, or re-emerging rust stains. Faced with these defects, the site foreman must not attempt cosmetic patch-ups using fine mortar: the intervention requires methodical analysis and immediate surgical remediation.
- Systematic hammer sounding: any reprofiled area sounding hollow indicates bond failure at the interface; total breakout of fresh or hardened mortar down to the sound substrate is mandatory.
- Passivation defect: persistent traces of oxidation require reopening the area, clearing the rebar around its entire perimeter, and repeating mechanical wire brushing before reapplying the anti-corrosion primer.
- Surface cracking: caused by thermal bridging or poor curing, this compromises impermeability; if adhesion is maintained, bridging via injection or suitable grout is specified following approval by the site management.
In accordance with CO, the contractor notifies the site management without delay of any unforeseen discovery during chipping, such as a rebar cross-section loss exceeding 20% or carbonation extending beyond initial limits. Collective safety during high-level breakout and heavy dust extraction are governed by the provisions of the Construction Work Ordinance.
Frequently asked questions
How should one respond if exposed rebar exhibits a reduced cross-section due to rust?
As soon as steel cross-section loss exceeds approximately 15 to 20%, stop local breakout and notify the appointed civil engineer. The contractor does not decide on structural reinforcement on their own initiative. In accordance with SIA 118, a non-conformity report is submitted to the site management. The engineer will calculate the requirement to weld supplementary bars, anchor new steels, or add composite plates prior to any reprofiling.
Can thixotropic mortar be placed onto a bonding bridge that has begun to set?
No, this is strictly prohibited. A hydraulic bonding coat must always be worked wet-on-wet. If the slurry forms a dry or matt skin under touch, it acts as a debonding layer preventing intimate bonding of the reprofiling mortar. This slurry must immediately be stripped by aggressive wire brushing or light chiselling, thoroughly dedusted with dry compressed air, and the bonding bridge reapplied immediately before the mortar.
What should be done when a hollow sound is detected with a hammer after full hardening?
A hollow sound reveals delamination between the existing concrete and the repair mortar. No surface resin can compensate for this structural void. You must saw-cut the defective boundary using an angle grinder to a depth of at least ten millimetres, then break out the entire patch with a light pneumatic chipping hammer. The surface is stripped again, saturated with water the day before, and reprofiled according to the original protocol under thorough protection against desiccation.
What emergency measure should be applied in the event of surface crazing after striking formwork?
Crazing indicates premature evaporation of mixing water, often linked to missing sheeting or draughts. First sound the element to verify that the mortar core has not debonded. If the material is dense and sound, immediately apply extended wet curing using soaked hessian kept continuously wet, then provide an approved anti-carbonation fairing coat validated by the site management.
Texts and standards cited
- COmaterial and site conditions: the contractor shall immediately inform the client of any circumstances compromising the proper execution of the works (para. 3)
- norme SIA 118general conditions for construction work