🧱 CFC 201 / 211.0Mortars, site-mixed concretes and placement productsChapter 10 of 10 in the section

Striking time: target strength and control test specimens

This chapter provides the method to determine the exact moment for striking formwork without risking spalling the edges or deflecting slabs. You will learn how to organise strength monitoring using site test specimens, manage curing conditions according to SIA 262 and formalise site management approval for the works file.

Key takeaways

  • Striking strength depends on the load-bearing function and immediate stresses on the element.
  • Site test specimens must be subjected to exactly the same thermal conditions as the actual structure.
  • Premature striking damages sharp edges and compromises the durability of fair-faced surfaces.
  • Formal authorisation from the engineer remains mandatory before removing props under a slab.

Determine minimum strength and manage fair-faced surfaces according to SIA 262

Removing wall formwork panels or soffit formwork too early exposes the structure to two major risks: mechanical degradation of surfaces and excessive deflection of load-bearing elements. For vertical walls, a strength between 2 and 5 MPa is generally sufficient to prevent material pull-out when stripping the formwork and to guarantee the integrity of corners. Conversely, for slabs or beams struck without heavy backpropping, the concrete must often reach 50 to 70% of its 28-day characteristic strength in order to support its own self-weight and construction site live loads.

Indicative strengths required prior to striking on the construction site
Structural elementPrimary stressTarget strengthRisk in the event of early removal
Walls and abutments (vertical formwork)Zero self-weight on the edge2 to 5 MPaCorner spalling, surface tearing
Slab soffits with immediate backproppingSelf-weight partially sustained10 to 15 MPaMicrocracking, shear cracking
Slabs and beams without load-transfer proppingTotal self-weight and service loads70% of final classExcessive residual deflection, structural defects
Cantilevers and overhangsMaximum bending moment at fixed support100% of design valueBrittle failure, irreversible sagging

Ambient temperature directly affects setting kinetics. In cold weather or when using low-heat cements, the usual summer striking times no longer apply. Using concrete maturity estimation through temperature monitoring allows the equipment rotation schedule to be adapted without compromising final quality.

Make site test specimens and record the written decision

Compliance of striking strength is not assessed on standard test specimens stored in water at 20 °C in the laboratory. To reflect the reality of the structure, the foreman prepares site test specimens kept at the exact location of the pour, under the same covers or thermal protections as the cast element.

  1. Sampling and compactionSample fresh concrete directly from the skip discharge or pump hose, then fill the cube moulds in successive layers compacted with an internal vibrator or tamping rod.
  2. On-site conditioningPlace the cubes immediately adjacent to the control element, under the same insulation or curing blankets, to ensure a strictly identical temperature history.
  3. Crushing in the pressCrush the cubes on a calibrated construction site press or in a testing laboratory at the agreed age (often 3 or 7 days) to validate the strength threshold.
  4. Submission of the test reportNotify the crushing result to site management and the responsible civil engineer to request the formal removal of props.

The written striking decision constitutes the key document in the works file. The site manager records the date, time of concreting, minimum overnight temperature, crushing value obtained and explicit authorisation from the design office. The contractor scrupulously respects its site management obligations under the Code of Obligations (CO), avoiding any unilateral initiative on load-bearing elements.

Each decentring operation is signed off in the site journal. The written record protects the masonry team in the event of subsequent disputes regarding deflections under partitions or floor cracking.

Striking protocols by element and risks to sharp edges

On a building construction site, striking time is not a matter of calendar routine but of a dual verification: the geometric integrity of the fair-faced surface and mechanical stability under self-weight. Removing formwork too early exposes the structure to two distinct types of damage. For vertical walls (walls, pillars), the major risk involves material tear-out, spalling of corners and surface scaling due to adhesion to the formwork skin. For slabs and main beams, the risk relates to irreversible deformation from early creep, or even partial failure of the structure.

The required striking strength varies according to the function of the formed element. Vertical panels carry no external vertical load during demoulding; they only require sufficient strength so that the concrete does not slump under its own weight and the edges do not chip when the panels are drawn back. Conversely, a slab soffit or beam must support its immediate self-weight as well as temporary construction site live loads from stored props or masonry pallets.

Indicative striking strength criteria by element type
Structural elementDominant stressMinimum target strengthRequired operation
Walls and shear wallsZero lateral pressure, risk of surface tear-out5 to 8 N/mm²Lateral striking with continued curing if necessary
Columns and abutmentsLow self-weight, handling impacts8 to 10 N/mm²Careful stripping of corners and chamfers
Medium-span slabsBending under self-weight and storey loads50 to 70% of fckStriking with immediate placement of drying props
Cantilevers and main beamsCritical tension / bending in the span75 to 85% of fckMaintaining full propping until inspection

For long-span slabs, striking does not mean the outright removal of all support. Backpropping — or the installation of drying props — must be carried out bay by bay without letting the slab deflect freely. The crew releases the jacks on the shoring towers or main props, removes the formwork panels, then brings relief props back into contact beneath the concrete without forcing with a jack, so as not to introduce unintended parasitic counter-stresses not accounted for in the structural design.

Decision chain, specimen crushing and traceability in the works file

Responsibility for the striking order follows a clear line: the contractor proposes the estimated date based on its records, but the written striking decision for flexural load-bearing elements rests with the civil engineer or site management, pursuant to the provisions of the works contract governed by SIA 118. Art. 364 CO sets out the contractor's general duty of care in executing the work, requiring the foreman to record all parameters influencing hardening.

  1. Sampling and curing of site test specimensPrepare 150 mm cubes or cylinders directly during pouring. Site test specimens are not placed in a moist room at 20 °C, but stored in the immediate vicinity of the element, under the same covers or thermal protections, to undergo strictly the same temperature history.
  2. Early crushing testTransport the specimens to the press in an on-site laboratory or third-party testing facility. Crushing at an intermediate age (e.g. 3, 5 or 7 days) provides the actual strength gained at the time planned for striking.
  3. Submission of the crushing test reportThe project manager immediately submits the strength certificate to site management and the civil engineer, together with ambient temperature records and the concreting log.
  4. Issuing the written striking approvalThe civil engineer formally validates the operation by email or sign-off in the site journal. Under no circumstances must striking of slab soffits or cantilevers begin based on simple verbal agreement from the foreman.

When construction site organisation precludes the use of specimens due to rapid cycle times, maturity sensors embedded in the concrete allow calculation of the liberated thermal energy and real-time estimation of equivalent mechanical strength. However, this correlation method requires prior approval from the civil engineer on the reference curve of the cement used.

Managing striking non-conformities and traceability

Premature or poorly controlled striking causes immediate defects: spalled edges, surface laitance tear-out or abnormal slab deflections. If crushed site test specimens fail to achieve the striking strength specified by the civil engineer, or if the element displays a critical visual defect, the team must immediately halt prop removal operations. The foreman logs the incident in the site journal and alerts site management.

  1. Logging and immediate backproppingStop striking. In the event of suspicious deflection or cracking, reinstall emergency propping without forcing beneath the affected element. Cordon off the area below.
  2. Joint inspection record and analysisConvene the civil engineer and site management to establish a joint inspection record on the nature of the damage: fair-faced appearance defect under SIA 262 or structural compromise.
  3. Formal remediation decisionStrictly implement the protocol prescribed by the engineer: extended curing, non-destructive surface hardness testing or edge repair using suitable thixotropic mortars.

The contractor is liable for the proper execution of the works. Art. 365 CO states that if circumstances compromise the regular or timely execution of the work, the contractor must inform the client. The written striking decision, approved by the civil engineer on the basis of crushing reports from specimens cured on site, constitutes the only acceptable supporting document to discharge the contractor and close the works file.

Frequently asked questions

What should be done if a sharp edge breaks cleanly off during formwork stripping?

Stop striking in that area. Keep the fragments and take photographs for the daily report. Check the striking strength achieved by the site test specimens. If the cause is mechanical, prepare the substrate by wire brushing and apply a non-shrink repair mortar specified by site management, following formal approval from the civil engineer.

Can striking be authorised without crushing specimens cured on site?

No, not for slabs and beams subjected to heavy loading immediately upon decentring. SIA 262 requires the actual in-situ maturity of the concrete to be verified. Standardised laboratory specimens do not reflect construction site temperatures. Without crushed site test specimens or a validated maturity measurement, the team leader cannot obtain the required written striking decision.

Who bears the final responsibility for ordering the removal of props?

The civil engineer sets the minimum required strength in their drawings and tenders. The foreman provides the physical evidence: crushing reports from site test specimens and curing temperature logs. The written striking decision is co-signed or issued by site management before any complete removal of propping from main spans.

How should an extended striking period be recorded in the works file?

Record the curing variation in the site journal, specifying recorded night temperatures and specimen results. Attach the calculation note or sign-off provided by the civil engineer. This documentary record proves compliance with the requirements of SIA 262 upon final handover of the structure.

Texts and standards cited

  • SIA 262Swiss technical standard on concrete structures and execution conditions
  • OTConst art. 17Protection against the collapse of construction elements or falling objects and materials: measures must be taken at workstations and passageways so that workers are not endangered.
  • CO art. 365Materials and ground: the contractor is liable for the good quality of materials supplied; if materials supplied by the client or ground designated by the client are found to be defective, or if any other circumstance compromises the regular or timely execution of the work, the contractor must notify the client immediately, under penalty of bearing the consequences (para. 3).

In the same section