🧱 CFC 250Drinking water: introduction, protection and meterChapter 4 of 10 in the section

Choosing materials: copper, stainless steel, multilayer and prohibited pairings

This chapter gives you the rules for joining drinking water distribution pipes according to the SSIGE guidelines. You will learn to identify incompatible metal pairings, to respect the installation direction to neutralise ion transport, to select approved transition fittings and to check the approval of materials in contact with drinking water.

Key takeaways

  • Installing copper upstream of galvanised steel destroys the steel through the transport of metal ions.
  • Galvanised steel must always be located upstream of components made of copper or copper alloys.
  • The SSIGE guidelines require the exclusive use of approved materials to preserve water hygiene.
  • Physical separation by dielectric fittings or bronze parts prevents contact corrosion.

Understanding galvanic corrosion and respecting the flow rule between metals

On renovation construction sites in French-speaking Switzerland, the meeting of existing galvanised steel risers with new copper or stainless steel distribution is one of the main causes of damage through perforation. Two distinct degradation mechanisms come into play when metals are mixed: galvanic contact corrosion and pitting corrosion induced by the ions carried in the water flow.

Contact corrosion appears when two metals with different electrochemical potentials are connected directly without an electrical insulator. In this galvanic couple bathed in conductive water, the less noble metal, the anode, undergoes accelerated dissolution to the benefit of the nobler metal, the cathode. The zinc of the galvanised steel and the iron itself sacrifice themselves in the face of copper or stainless steel. The exchange surface acts as a critical amplifier: a small anodic surface connected to a large cathodic surface leads to local perforation within a few months.

Behaviour of metal assemblies according to flow direction
Upstream materialDownstream materialDirect connectionConnection with insulator / bronze
Galvanised steelCopperProhibited (contact corrosion)Compliant (flow rule respected)
CopperGalvanised steelProhibited (rapid perforation)Prohibited (destructive ion transport)
Stainless steelCopperTolerated depending on gradeCompliant with threaded intermediate piece
Galvanised steelStainless steelProhibited (galvanic corrosion)Compliant with dielectric insulating sleeve
Synthetic multilayerAny metalCompliant (neutral material)Compliant with SSIGE-certified fittings

The plumber must analyse the entire installation before intervening. If a valve, a check valve or a section of copper pipe is located upstream of a galvanised pipe that is being kept, the water will carry the corrosive ions to the latter. The unchanging order from upstream to downstream must progress from the least noble metal to the noblest: first galvanised steel, then brass or bronze, then copper, and finally stainless steel or synthetic materials.

Installing transition fittings and ensuring SSIGE approval

Managing the interfaces between materials requires rigorous jointing methods in order to meet the requirements of the SSIGE guidelines on drinking water installations. The transition between two pipes of different types must never create a direct contact couple nor degrade the quality of the water supplied. The components used must appear in the register of certificates of the Swiss Gas and Water Industry Association.

  1. Diagnosis of the existing upstream sectionScrape the outside of the pipe and check the internal condition if a cut is made. Identify the presence of galvanised steel, cast iron or prohibited lead, and measure the actual nominal diameter before ordering the parts.
  2. Inserting an intermediate spacer pieceTo connect upstream galvanised steel to a downstream copper or stainless steel network, fit a separation piece made of bronze or dezincification-resistant brass, with a minimum length equal to twice the nominal diameter.
  3. Fitting a dielectric fitting on a live networkWhere there is a risk of stray currents or parasitic electrical potentials transmitted by equipotential bonding, install an insulating flange or a certified dielectric sleeve with a ring made of synthetic material.
  4. Checking sanitary approvalsCheck that every fitting, isolating valve, elastomer seal and multilayer pipe has its SSIGE certificate number, valid for direct contact with drinking water.

Multilayer pipe, made of laser-welded aluminium lined with cross-linked polyethylene, is today the preferred technical solution for floor branches and appliance connections. Chemically inert, insensitive to galvanic corrosion and providing a total barrier against oxygen penetration, it eliminates any electrochemical risk when tying into metal networks. The press fittings must nevertheless be chosen from the same system approved by the manufacturer to guarantee long-term watertightness.

Where a modification requires supplying a galvanised section downstream of a modern installation, complete replacement of the galvanised section with stainless steel or synthetic material is the only lasting measure. Under the Code of Obligations (CO), the installer informs the client of any defects or incompatibilities in the existing material in order to prevent foreseeable damage.

Domestic hot water loop and galvanised steel: the trap of the return in a mixed network

The domestic hot water (DHW) circulation loop is the most destructive failure case encountered in partial refurbishments in French-speaking Switzerland. Although the fitter scrupulously respects the flow rule on the distribution network by placing the zinc-coated steel upstream and the copper or multilayer pipes downstream, the return circuit physically reverses this logic. Hot water that has passed through pipework or valve bodies made of copper alloy becomes loaded with soluble cupric ions. On re-entering the water heater or when connected upstream of a galvanised steel riser, this water carries noble elements that deposit directly on the zinc surface.

Compatibility of metal assemblies in sanitary distribution (according to SSIGE W3 guidelines)
Upstream materialDownstream materialNetwork without loop (one-way)Network with DHW loopMandatory installation measures
Galvanised steelCopperPermittedProhibitedInterpose a non-magnetic separation piece or a certified bronze fitting.
CopperGalvanised steelStrictly prohibitedStrictly prohibitedTotal electrochemical incompatibility: risk of rapid perforation by pitting.
Stainless steelCopperPermittedPermittedUse approved press or threaded fittings to avoid any direct couple.
Galvanised steelStainless steelPermittedProhibited if returning onto steelDirect connection tolerated in a cold network provided the flow direction is respected.
Multilayer (PEX/Alu)All metals permittedPermittedPermittedThe aluminium core remains isolated from the water by the inner polyethylene layer.

To neutralise this danger permanently when modernising a floor distribution, the installer must galvanically isolate the renovated sections. If the original zinc-coated steel manifold or riser is kept, the connection to a copper or multilayer branch is made by means of an intermediate fitting in bronze or dezincification-resistant brass, supplemented if necessary by a dielectric insulating sleeve. On the other hand, if a circulation loop is kept in service, the loop network must under no circumstances be converted to copper if the risers remain galvanised steel. In this configuration, complete replacement of the loop with stainless steel or certified synthetic material is required to ensure the installation's longevity.

SSIGE certification and installation of approved materials in contact with drinking water

In Switzerland, the selection of components for an internal sanitary installation does not depend solely on mechanical or pressure-resistance criteria. Any product coming into contact with water for human consumption must comply with the sanitary and hygiene requirements defined by the Swiss Gas and Water Industry Association. The SSIGE W3 guidelines require that all pipework, shut-off valves, fittings and safety devices come from ranges tested and listed in the public register of SSIGE Water certificates. This approval attests that the materials release no toxic substances into the network and do not promote bacterial growth.

  1. Checking markings on delivery to the construction siteVisually check that every bar, coil of multilayer pipe and box of fittings bears the official SSIGE stamp and the pressure class reference (PN 10 or PN 16). Reject immediately any imported batch without a valid Swiss certificate.
  2. Selecting interface connection piecesUse exclusively junction pieces made of silicon bronze, compliant traditional bronze or approved synthetic material to provide the mechanical interface between dissimilar metals.
  3. Cutting and calibrated deburringCut the pipes with a pipe-cutting wheel or the pipe cutter specific to the material. Carry out careful internal and external deburring with a rotary deburring tool to remove loose metal swarf that would form starting points for local galvanic corrosion.
  4. Pressure flushing and filling with water without stagnationFlush the pipe intensively in accordance with the SSIGE W3 guidelines before final commissioning. Never leave a new installation filled with stagnant water without regular draw-off during the finishing work phase.

From a contractual and legal standpoint, the contractor remains responsible for the conformity of the work and the quality of the materials it supplies and incorporates into the building. In the event of manifest non-compliance with the SSIGE technical guidelines or the use of incompatible alloys causing recurrent water damage, the plumber's liability is directly engaged on the basis of the contract-for-work rules set out in the Code of Obligations (CO). Rigorous checking of suppliers' data sheets and absolute mastery of metal combinations are the only safeguards against premature defects.

Remediation protocol in case of active corrosion or reversed installation

The discovery of perforating corrosion pits or brownish discolouration of the water in a mixed sanitary installation signals an active electrochemical incompatibility. In the event of water damage or a perforation on a galvanised steel pipe located directly or indirectly downstream of copper components, a makeshift seal with a repair sleeve solves nothing: the migration of cupric ions will continue to destroy the protective zinc and the base metal at every draw-off.

  1. Isolate the network and lock out the distributionClose the upstream isolating valve, drain the affected riser and lock out the pipe. If the building remains occupied, set up a temporary supply in SSIGE-certified multilayer pipe to guarantee continuity of drinking water without risk of contamination.
  2. Trace the hydraulic path and identify the reversalSurvey the entire cold and domestic hot water layout, without overlooking any loop returns. Examine the order of the metals according to the actual direction of circulation: identify every copper component located upstream of zinc-coated steel pipes.
  3. Remove the affected section and restore the materialRemove the galvanised steel pipes attacked by pitting. Replace the degraded pipes with compatible materials insensitive to the phenomenon: stainless steel or SSIGE-approved multilayer. If the upstream copper remains, the entire downstream section must absolutely abandon galvanised steel.
  4. Flush, test and record the technical fileAfter compliant assembly of the transition fittings, carry out intensive flushing to remove residual ferrous oxides. Carry out the pressure test in accordance with the SSIGE W3 guidelines, then update the installation diagram handed to the site management.

Any refurbishment requires strict vigilance regarding the components installed: every pipe, valve and transition fitting must appear in the register of materials certified by the SSIGE for contact with water for consumption. If the network already shows generalised corrosion, the plumbing foreman must notify the defect to the client and recommend complete replacement of the non-compliant section.

Frequently asked questions

Can a cold water copper pipe be connected downstream of an old galvanised steel pipe?

Yes, in this specific flow direction the arrangement remains compliant with the SSIGE W3 guidelines. As the galvanised steel is upstream, the iron or zinc ions carried by the fluid do not affect the copper placed downstream. The installer must nevertheless make sure to fit a transition fitting in bronze or dezincification-resistant brass in order to prevent direct contact corrosion at the assembly thread.

Does a dielectric insulating fitting protect galvanised steel placed after a water heater connected in copper?

No, the dielectric fitting only cuts the passage of electric current through direct contact between the metals. Downstream of a pipe or appliance containing copper, the water dissolves traces of cupric ions. These ions migrate with the flow and react directly with the zinc coating of the galvanised pipes. This chemical reaction causes rapid local perforation, making the dielectric fitting completely ineffective against this type of corrosion.

How can you check whether a fitting or multilayer pipe is approved for drinking water in Switzerland?

The installer must check the physical marking of the product and consult the SSIGE online register. Approved components bear an explicit stamp with the SSIGE label and a valid certificate number. Installing unlisted components on the drinking water distribution network exposes the company to rejection at acceptance during inspection of the installation and to the obligation to replace everything at its own expense.

Why do mixed installations with a hot water circulation loop pose an increased risk?

In a domestic hot water loop, the water circulates in a continuous closed circuit. Even if the outgoing flow appears to respect the theoretical flow order, the return pipe re-injects the fluid loaded with metal ions towards the upstream of the system. If the loop contains copper and galvanised steel, the copper ions inevitably end up coming into contact with the zinc-coated parts, initiating accelerated galvanic degradation throughout the hot water loop.

Texts and standards cited

  • Directives SSIGE W3Guidelines for drinking water installations (W3): design principles, choice of materials and corrosion protection

In the same section