Preloaded joint: preparation of friction surfaces and slip factor obtained

This chapter details the execution requirements to guarantee the slip factor in preloaded joints. You will learn how to define and inspect workshop grit blasting, apply rigorous masking to prevent any coat of paint at the joint, and inspect the condition of contact faces before final tightening on the construction site.

Key takeaways

  • The calculated slip factor depends directly on the mechanical preparation applied to the steel.
  • Any trace of paint or primer is strictly prohibited on the contact area.
  • Workshop masking must precisely cover the joint perimeter to prevent excess thicknesses.
  • SN EN 1090 requires a rigorous visual inspection before final tightening of preloaded bolts.

Prepare roughness in the workshop and prohibit contaminating coatings

In a slip-resistant preloaded joint, the shear force does not pass through the bolt shank in contact with the hole wall. Transmission occurs exclusively through friction mobilized between the steel faces firmly pressed together by the preloading of the bolts. Consequently, the surface condition directly governs the structural safety of the node. Any degradation of the metal relief reduces slip resistance and compromises the overall behaviour of the steel structure.

The standard SN EN 1090 defines the required surface classes according to the civil engineer's calculation notes. To achieve the highest slip factors, the benchmark treatment remains blasting with angular abrasive, commonly referred to as grit blasting. This process completely removes mill scale, oxides and dirt to generate a uniform, sharp roughness. White metal or near-white metal grit blasting provides an ideal surface for microscopic interlocking of the faces under the action of preloading.

Surface treatments and indicative slip factors according to execution standard SN EN 1090
Applied treatmentSurface classIndicative slip factorSpecific workshop requirement
Grit blasting with angular abrasive without paintClass A0.50Immediate protection against ambient humidity
Grit blasting then spray application of zinc silicateClass B0.40Strictly controlled dry film thickness
Vigorous wire brushing free of mill scaleClass C0.30Total removal of loose rust
As-rolled untreated steelClass D0.20Absolute absence of grease or non-adherent mill scale

Fabrication planning must incorporate this rule even before parts enter the paint booth. If a shop primer is sprayed over a friction-grip joint area without prior precautions, subsequent manual stripping on the construction site by grinding will never restore the initial grit-blasted texture. The steel fabricator must ensure paint operators comply with these specifications, otherwise incurring liability under art. 364 CO, which provides that the contractor is liable for the proper and faithful execution of the work assigned.

Master workshop masking and inspect faces before tightening

Achieving a compliant joint relies on the rigorous marking out of contact surfaces right from the workshop marking-out stage. To prevent any overspray infiltration during the application passes of anti-corrosion systems, splice plate areas and end plate faces must receive robust masking that withstands solvents and curing temperatures.

  1. Locating connection templatesDetermine from the execution drawings the exact area covered by cover plates, end plates or shims, incorporating a minimum safety margin of ten millimetres beyond the outer overlap perimeter.
  2. Applying heavy-duty adhesive tapesApply technical cloth tape or specific industrial spray booth tape directly onto the grit-blasted plate, ensuring continuous adhesion without wrinkles or edge lifting.
  3. Fitting sacrificial steel cover platesFor elements stored temporarily outdoors or undergoing heavy handling, bolt false steel plates over the connection holes to physically block any paint deposits or accidental overspray.
  4. Unmasking and integrity inspectionRemove adhesive protections immediately after thorough curing of the anti-corrosion coating to prevent adhesive residue transfer onto the grit-blasted steel.

On the erection construction site, the erection foreman visually checks each contact surface before assembling the components. Bare blasted steel is vulnerable to weather. Light surface rust of a reddish shade, known as flash rust, generally does not alter Class A friction provided it does not form corrosion pits or loose flakes. In contrast, mud deposits, formwork oil traces, rigging grease or frost must be removed using a non-rotary wire brush or by degreasing with a clean solvent leaving no waxy residue.

The inspection report records the check of the surface condition, the batch of grit-blasted components and the date of masking removal. Assembly of parts must follow a tight schedule: a joint closed promptly prevents contamination of internal faces by construction site dust and water ingress before application of the final preloading torque.

Friction classes according to standard SN EN 1090-2 and obtained roughness

In a slip-resistant preloaded joint, the shear force does not pass through the bolt shanks acting in direct shear, but through the friction generated between the plates clamped under the preloading effect. The design of these nodes depends entirely on the friction class selected by the civil engineer on the execution drawings. The standard SN EN 1090 imposes a strict correspondence between the mechanical or chemical treatment applied to the contact surfaces and the design slip factor taken into account in the ultimate limit state calculations.

Classification of contact surfaces and slip factors according to standard SN EN 1090-2
Friction classNominal slip factor (µ)Surface treatment required in workshopVisual inspections and roughness
Class Aµ = 0.50Grit blasting or shot blasting to grade Sa 3 with sharp surface profile, free of rust and mill scale.Total absence of dust, average roughness conforming to reference specimens.
Class Bµ = 0.40Grit blasting or shot blasting to grade Sa 2½ followed by certified thermal spray zinc or aluminium metallisation.Uniform layer without blistering, sealing coats prohibited on the mating face.
Class Cµ = 0.30Cleaning by vigorous wire brushing or flame cleaning, or grit blasting without sharp profile.Bare metallic surface, traces of adherent surface oxidation conditionally tolerated.
Class Dµ = 0.20As-rolled untreated steel, cleared of loose mill scale flakes.Dry and degreased plates, free of anti-rust treatment or primer coat.

Angular metallic grit blasting is the standard method to achieve Class A. Round shot produces peening without sharp edges, unable to generate the micro-mechanical interlocking effect required during controlled torque tightening. When the designer specifies Class A or B, the steel fabricator must ensure that the abrasives used in the treatment booth guarantee an adequate peak profile. Any deviation from the specified treatment immediately reduces the load-bearing capacity of the joint and invalidates the structural analysis.

Marking out contact areas, lap tolerances and remediation on the construction site

Managing the geometric boundaries of the friction surface begins right from the tracking on fabrication drawings. The area free of any paint coat is not limited to the exact footprint of the washer or splice plate. The paint prohibited within the joint extends across the entire area covered by splice plates, plus a continuous perimeter clearance strip. Technical adhesive tape resistant to abrasive blasting defines the footprint before passage into the paint booth.

  1. Setting up masking in the workshopPosition reinforced adhesive tapes or magnetic steel templates extending at least 15 mm beyond the theoretical perimeter of the splice plate or connecting flange plate.
  2. Inspection after applying the anti-corrosion systemRemove masking as soon as the film surface dries to avoid tearing edges. Confirm the absence of burrs or runs within the friction area.
  3. Packaging and transportApply watertight temporary protective sheets or spacers to protect bare blasted metal from water splash, de-icing salts and greasy contamination during transport to the construction site.
  4. Inspection prior to final assembly on siteVisually inspect for the absence of loose powdery oxidation. In the event of accidental contamination by lifting oil, degrease using a volatile solvent that leaves no oily residue.
  5. Mechanical remediation in case of contaminationIf paint has run into the clamping surface during touch-ups on the construction site, prohibit torch burning. Proceed exclusively with localized dry grit blasting or mechanical sanding using a clean abrasive disc until the bare metallic profile is restored.

During erection, site foremen must coordinate operations so that preloaded connections are closed and tightened promptly after unpackaging the components. Prolonged exposure of grit-blasted steel to weather leads to the formation of non-adherent oxides likely to alter the slip factor. Pursuant to art. 364 CO, the contractor is liable for the careful management and execution of these operations according to the recognized rules of the steel trade. If a surface exhibits a defect non-compliant with specifications, full remediation is mandatory prior to any final torque tightening, thereby ensuring the structural durability of the works under dynamic loads.

Managing surface non-conformities and remediation on the construction site

On a structural steelwork construction site, the discovery of paint, anti-corrosion primer or greasy mill scale at a preloaded node calls for an immediate halt to tightening. In a friction joint, the transmission of transverse loads relies exclusively on mechanical grip between the faces clamped by the HR or HV bolt assembly. The presence of an uncertified paint film lubricates the contact, drastically reduces slip resistance and induces creep under permanent axial load, which eliminates the initial bolt preload.

When visual inspection reveals a masking error made in the workshop or touch-up paint bleed, the site foreman applies a rigorous remediation procedure before any final assembly. Using an angle grinder equipped with a rough grinding disc is strictly prohibited, as it glazes the steel and lowers the slip factor. Remediation requires targeted thermal stripping or mobile pneumatic micro-grit blasting to restore the cleanliness level and roughness specified by standard SN EN 1090-2.

  1. Marking out and paint removalMark out the theoretical contact area with a 10 mm margin beyond the washers. Completely strip the paint film or oil residues using a non-oily degreasing solvent, followed by mechanical wire brushing or localized grit blasting.
  2. Restoring the roughness profileRecreate the required anchor profile by open-blast grit blasting on the construction site or via a certified rotary needle tool, without polishing the metal. Visually inspect for the total absence of residual binder traces or dust before presenting splice plates.
  3. Recording and conformity checkMeasure the obtained surface roughness using a surface profile gauge or visual-tactile comparator. Record the operation and the measured parameters in the erection log in accordance with execution traceability requirements.

If the client observes a structural non-conformity relating to a joint executed on a non-compliant painted surface, CO para. 2 applies: the client may set a time limit to rectify the defective execution and have the work redone at the contractor's expense. Complete dismantling, compliant stripping and mandatory replacement of preloaded bolts already tightened then become compulsory.

Frequently asked questions

Can a thin coat of shop primer be tolerated on contact faces?

No. Unless justified by a slip test report specific to the applied product, standard paint or anti-corrosion primer is strictly prohibited on friction surfaces. A standard paint film degrades and creeps under the colossal pressure exerted by controlled tightening. It leads to a rapid loss of preload in the bolt assembly and ruins the safety of the preloaded joint under shear loads.

How should a rusted friction surface be treated after storage on the construction site?

Non-adherent surface rust can be removed using a clean hand wire brush, without rubbing the steel to a shine. If corrosion has produced pitting or loose mill scale, localized grit blasting is required to restore a sound surface. The presence of fatty substances combined with rust requires full degreasing with clean solvent prior to any mechanical brushing, to avoid embedding oil into the microporosities of the steel.

Why must preloaded bolts removed to rectify a surface be replaced?

HR or HV bolts tightened to torque or using the combined method undergo controlled plastic deformation in the thread and shank. In the event of dismantling a joint to strip a surface painted by mistake, standard SN EN 1090-2 prohibits the reuse of these fasteners. Bolts, nuts and washers that have already been preloaded must be scrapped and replaced with new components from a uniform and originally lubricated assembly lot.

Which masking method guarantees the absence of paint during coating application?

The steel fabrication shop applies heavy-duty adhesive tapes specific to powder coating or steel templates bolted directly to the holes before grit blasting and painting. The reserved areas must cover the entire contact surface beneath the splice plate with an overlap of at least 10 millimetres beyond the outer perimeter of the washers. Masks are removed after full curing to preserve clean paint edges without runs.

Texts and standards cited

  • SN EN 1090-2Execution of steel structures and aluminium structures - Technical requirements for steel structures (contact surfaces, friction classes and tightening of preloaded joints)
  • CODelay and foreseeable defective execution: setting of a time limit by the client to repair or continue the work at the contractor's expense and risk (para. 2)