Key takeaways
- Wind blows shielding gas away and requires a tight shelter even in light breezes.
- Ambient humidity or condensation introduces hydrogen and risks causing cold cracking.
- Preheating steel is required based on thickness and carbon equivalent to slow cooling down.
- Standard SN EN 1090 requires strict adherence to Welding Procedure Specifications on site.
Gas shielding and draught management on the construction site
Gas-shielded arc welding (MAG or TIG processes) is extremely sensitive to ambient air. On a steelwork construction site, a simple draught deflects the flow of inert or active gas. Without this protective cover, oxygen and nitrogen in the air come into contact with the weld pool. This causes immediate porosity in the weld bead, oxide inclusions, and a drastic loss in the mechanical properties of the joint.
To ensure joint conformity on site, setting up a welding shelter is not an option for comfort but a technical necessity. Tarpaulins and temporary booths must tightly seal the joint area. When wind exceeds the tolerances permitted by the Welding Procedure Specification (WPS), the crew must switch to a process less sensitive to air disturbances, such as manual metal arc welding (MMA) or gasless flux-cored wire welding.
Welding must be protected against wind, rain, and snow. Joint areas must be free of moisture, condensation, ice, rust, and grease before operations begin.
SN EN 1090-2
Humidity, cold cracking risk, and steel preheating
Water present on steel parts—in the form of rain, dew, or condensation—forms hydrogen during dissociation under the electric arc. This atomic hydrogen dissolves into the weld metal. During rapid cooling of the structure, trapped hydrogen migrates to stressed areas of the Heat-Affected Zone (HAZ), resulting in delayed microcracks, known as cold cracking. In accordance with art. 3 OPA, the employer takes safety measures adapted to the state of the art to prevent these structural risks.
- Preheating
- Thermal input applied to the steel component before and during welding, intended to slow the cooling rate, promote hydrogen outgassing, and avoid the formation of brittle martensitic structures.
The preheat temperature is determined based on the carbon equivalent of the steel, the thickness of the flanges or webs to be joined, and the heat input. Systematic drying with a torch is required to remove the surface moisture film, even if the metal appears dry to the naked eye.
| Combined thickness at the joint | Ambient humidity condition | Minimum required temperature | Prior action |
|---|---|---|---|
| Less than 20 mm | Dry air / Absent | 15 °C (Ambient temperature) | Mill scale cleaning |
| 20 to 40 mm | High relative humidity | 75 °C to 100 °C | Full drying with torch |
| Over 40 mm | Outdoor construction site / Cold | 125 °C to 150 °C | Pyrometer-monitored preheating |
Site welding requirements according to standard SN EN 1090
Moving from workshop fabrication to site assembly radically transforms weld quality control. Under standard SN EN 1090, executing welded joints in structural steelwork demands rigorous implementation of the welding procedure specifications (WPS). On the construction site, climatic deviations (high winds, precipitation, or low temperatures) alter arc stability and steel metallurgy, prohibiting any improvised tack welding without prior workstation preparation.
The erection environment directly influences bead geometry and soundness. While a workshop provides a controlled atmosphere, the construction site demands continuous vigilance regarding air speed directly at the joint and the moisture level of the component to be joined. Complying with fit-up tolerances requires the use of inspection methods suited to actual access at height or on composite façades.
| Environmental factor | Direct impact on the joint | Mitigation measure on the construction site |
|---|---|---|
| Wind > 2 m/s (MAG process) | Shielding gas blown away, porosities, and slag inclusions | Erection of windbreak sheets or switching to process 111 (MMA / covered electrode) |
| Ambient humidity and condensation | Diffusible hydrogen input, cold cracking in the HAZ | Torch drying and systematic preheating of the area |
| Low steel temperature (< 5 °C) | Ultra-rapid cooling, stiffening, and brittle fracture | Maintaining adequate interpass temperature and preheating |
Preheating control and construction site shelter setup
Moisture on bevels promotes hydrogen absorption by the molten metal, generating delayed microcracks in the heat-affected zone (HAZ). To counter this phenomenon on heavy structural steels or thick sections, preheating becomes mandatory. The preheat temperature is determined based on the combined thickness of the joint, the carbon equivalent of the steel, and the heat input of the root passes.
- Cleaning and eliminating condensationMechanically wire-brush bevels to remove mill scale and rust. Run the heating torch to vaporise the surface water film over a width of at least 75 mm on either side of the joint preparation.
- Preheating and temperature monitoringBring the component up to temperature according to the instruction sheet specifications. Check the reached value using temperature-indicating crayons or a calibrated infrared pyrometer on the face opposite heating.
- Protective cocoon erectionErect a temporary enclosed shelter using flame-retardant tarpaulins stretched over a rigid frame to block draughts beneath the walkway or floor decking.
- Controlled cooling managementOnce welding is complete, wrap the welded area in thermal wool insulating blankets to slow the temperature drop and avoid thermal shock.
Erecting a rigid shelter over the joint workstation is not a matter of comfort, but a technical requirement to stabilise the gas mixture flow rate. In accordance with general prevention rules set out in art. 82 LAA, the employer implements protective installations adapted to weather conditions. Likewise, according to OTConst, organisational and equipment measures are mandatory to safeguard the health of welders working while exposed to bad weather or severe cold.
Managing variances on the construction site and reworking defective welds
On a steelwork construction site, the emergence of welding defects caused by climatic conditions demands strict intervention. When visual or non-destructive testing reveals blowholes caused by loss of gas shielding in the wind, or microcracks induced by cold cracking in damp steel, welding must be stopped without delay. The workshop offers stable conditions, but on the construction site, the absence of a weatherproof shelter or insufficient preheating immediately compromises the integrity of the load-bearing joint.
Standard SN EN 1090 governs execution requirements for steel structures and defines execution classes (EXC1 to EXC4). In the event of climatic drift on the construction site (gusts disrupting the argon/CO2 flow or sudden temperature drops in the component), the site foreman must adapt welding procedures (WPS). If environmental conditions no longer allow the required preheat temperature to be maintained according to section thickness or if humidity levels cause continuous condensation on the bevels, joint welding operations must be suspended.
- Interruption and securing of the areaStop the operation as soon as wind speed disrupts the weld pool or rain infiltrates. Install reinforced tarpaulins or set up a weatherproof protective airlock.
- Examination and gouging of the defectRemove the contaminated or cracked zone by grinding or air-arc gouging. Inspect the root of the groove using penetrant testing or magnetic particle inspection to verify complete defect removal.
- Drying and rework preheatingDry the area with a torch, reapply the prescribed preheat temperature checking with a thermal crayon or infrared pyrometer, then execute the repair according to the qualified WPS.
If it is impossible to achieve the required quality on site due to a non-conforming substrate or severe bad weather, the contractor refers to the general duty of warning to the client. Under the Code of Obligations (CO), the site foreman records each interruption linked to wind or humidity in the site logbook to justify adjustments to the steel frame erection schedule.
Frequently asked questions
How can shielding gas be maintained in moderate wind on a boom lift?
In the presence of draughts, MIG/MAG shielding gas is swept away, leading to bead porosity. It is essential to erect a rigid windbreak screen or a welding tent around the connection node. If the shelter is insufficient, switch temporarily to self-shielded flux-cored wire or manual metal arc welding, subject to approval by the engineering design office and compliance with standard SN EN 1090.
What is the reliable method for measuring preheat temperature on site?
Measurement is taken on the side opposite the heat source or at a distance of at least four times the thickness of the component after withdrawing the flame. Sharp-melting temperature-indicating crayons or a calibrated infrared pyrometer are used. Preheating prevents rapid cooling of the parent metal and disperses moisture, thereby reducing the risk of cold cracking.
Can structural steelwork be welded under light rain beneath a temporary shelter?
Yes, provided that the weld joint and adjacent areas are completely free of water and condensation. The shelter must prevent any direct runoff. Before striking the arc, the joint area must be heated to approximately 60 °C to 100 °C with a torch to evaporate the surface water film and avoid hydrogen absorption into the weld metal.
Who is responsible for validating repairs of cracked welds on the construction site?
The welding coordinator (IWE/IWT) designated for the construction site reviews non-destructive testing reports (dye penetrant, ultrasonic, magnetic particle testing) carried out by a qualified testing body. They validate the repair procedure (rework WPS) prior to any grinding or buttering/surfacing. The site manager then records the operation in the as-built documentation in accordance with standard SN EN 1090.
Texts and standards cited
- SN EN 1090Execution of steel structures and aluminium structures - Technical requirements for steel structures
- COMaterials and ground: obligation to inform the client immediately if any circumstance compromises the orderly execution of the work