Key takeaways
- The choice of intumescent paint thickness is strictly determined per profile and not by overall surface area.
- The section factor Am/V characterises the rate of temperature rise of a steel profile exposed to fire.
- The required fire resistance rating determines the minimum dry film thickness to be applied.
- Thickness checks using a wet film comb and magnetic gauge validate the execution inspection report.
Calculating the section factor and factoring in fire resistance
To ensure the fire protection of a steel structure, the selection of the intumescent system is not based on an average coverage per square metre. The dry film thickness applied depends directly on the specific profile and its exposure to flames. The key geometric parameter is the section factor, expressed by the ratio Am/V (or Ap/V). In this formula, Am represents the steel surface area exposed to fire per unit length (in m⁻¹), while V denotes the volume of steel per unit length, i.e. the cross-sectional area of the profile. A very slender and extensively exposed profile has a high section factor: it heats up very rapidly and requires a thicker intumescent coat to maintain its load-bearing capacity.
- Section factor (Am/V)
- Ratio between the steel surface area exposed to flames and the total volume of the profile per linear metre, measured in m⁻¹. It determines the rate of temperature rise of the profile in the event of fire.
In addition to profile geometry, the required fire resistance rating for the structure (for example R 30, R 60, or R 90) defines the duration during which the structure must retain its mechanical properties below the critical steel temperature (generally set at 500 °C or 550 °C by the structural engineer). For the same resistance rating, a massive IPE 500 beam will not require the same quantity of paint as a slender, thin-walled hollow section. The site manager must ensure that each profile type on the working drawing is paired with its specific section factor data sheet.
Using manufacturer tables, thickness inspection, and the inspection report
The steelwork contractor relies on the supplier's table specific to the intumescent product certified under VKF/AEAI approval. By cross-referencing the calculated section factor (Am/V), the number of exposed sides (3 or 4 sides), the chosen critical temperature, and the required R rating, the table indicates the required nominal dry film thickness (DFT), generally expressed in micrometres (µm).
- Recording wet film thickness (WFT)During application in the workshop or on the construction site, continuously monitor the fresh thickness using a graduated measurement comb to adjust the passes of the airless spray gun.
- Measuring dry film thickness (DFT)After complete drying, perform non-destructive measurements using a magnetic or eddy-current thickness gauge on each structural member.
- Applying the tolerance ruleVerify that the average of the measurements complies with the specified DFT. Individual tolerated values must not fall below the threshold permitted by the product approval (often 80% of the required thickness).
- Drafting the execution inspection reportRecord all measurements per profile, paint batch numbers, atmospheric conditions during application, and sign the fire protection labelling declaration.
The inspection and inspection report constitute the official documentation submitted to site supervision and the fire protection authority to obtain the occupancy permit. Under the Code of Obligations (CO), the contractor is responsible for delivering work that complies with technical specifications. As part of work organisation, the employer takes the measures required by the accident prevention ordinance to ensure the health protection of painters, particularly through suitable ventilation and the wearing of personal protective equipment when spraying solvent-based products.
Any steel structure protected by an intumescent system must be covered by an inspection report certifying that the average applied thickness meets the approval requirements for the profile concerned.
AEAI fire protection guideline / Construction site guidelines
Determining dry film thickness according to profile massivity
The thickness of an intumescent paint intended for the fire protection of a steel frame is never estimated per square metre of painted surface or using an overall lump-sum approach. In steel construction and composite facades, the quantity of dry film required to ensure structural stability depends directly on the section factor of the steel profile, designated as Ap/V (or Am/V), expressed in inverse metres (m⁻¹). This essential geometric ratio corresponds to the profile surface area directly exposed to the heat flux of the fire divided by the corresponding steel volume. A slender profile with a high section factor heats up very quickly in a fire event, as its low steel mass absorbs heat energy poorly. Consequently, it requires a significantly thicker coat of intumescent paint than a massive member to maintain the fire stability required by the building's fire safety concept.
| Profile type | Exposure | Ap/V factor (m⁻¹) | DFT for R 30 (µm) | DFT for R 60 (µm) | DFT for R 90 (µm) |
|---|---|---|---|---|---|
| HEB 300 | 4 sides | 115 | 280 | 550 | 1120 |
| IPE 300 | 4 sides | 215 | 420 | 1050 | 2100 |
| HEA 200 | 3 sides (slab) | 190 | 380 | 920 | 1850 |
| Hollow section 100x5 | 4 sides | 260 | 510 | 1380 | 2650 |
To determine the dry film thickness (DFT) to apply to each member, the site manager and the foreman cross-reference three fundamental parameters: the target fire resistance class (for example R 30, R 60, or R 90), the critical temperature assigned to the steel member by the structural specialist (generally between 500 °C and 600 °C depending on the mechanical stress ratio), and the section factor specific to the member. The contractor then refers to the official approval table provided by the manufacturer of the certified intumescent product. A common error on construction sites is applying the same schedule to a column exposed on 4 sides and to a beam in contact with a concrete slab exposed on 3 sides. This distinction alters the section factor value and can lead to a critical shortfall in thickness in an actual fire event.
Thickness inspection, tolerances, and drafting the inspection report
The intumescent paint system forms an indivisible assembly comprising the anti-corrosion primer base, the intermediate intumescent coat, and the aesthetic sealing topcoat. On the construction site as well as during workshop operations, the contractor is subject to strict execution requirements governed by the Code of Obligations (CO). The site manager verifies the chemical compatibility between the existing anti-rust primer and the specified intumescent system. Any incompatibility between the primer and the intumescent product risks causing surface crazing or loss of adhesion during the expansion of the protective foam upon contact with heat.
- Continuous monitoring of wet film thickness during applicationDuring airless spray passes, the applicator painter checks the wet film thickness using a stainless-steel comb gauge. This immediate check allows prompt adjustment of the gun speed to achieve the theoretical dry film thickness once solvent evaporation is complete.
- Magneto-inductive measurement of cross-linked dry film thicknessAfter through-drying of the product, dry film thickness is measured on the ferromagnetic steel substrate using an electromagnetic magneto-inductive gauge calibrated on precision shims. Readings include systematic measurements on the top flange, bottom flange, and web of profiles.
- Drafting and transmission of the quality assurance inspection reportThe foreman summarises all readings on an official quality assurance inspection report. This document records member identification, product reference, batch numbers, calculated section factor, specified DFT, and measured average. This inspection report is submitted to site supervision and inspection authorities to validate structural compliance.
Managing out-of-tolerance areas and compilation of the as-built application report
During the dry film thickness (DFT) inspection of the intumescent system on the steel frame, identifying undersized areas directly compromises the targeted fire resistance rating (R30 to R120). Compliance of the protection is not assessed across the overall square meterage, but profile by profile, by measuring the applied thickness against the section factor Ap/V specific to each steel cross-section. A massive profile requires less thickness than a slender profile, but a local thickness deficiency on an IPE flange or a HEB column results in the immediate rejection of the work during the acceptance inspection by the fire safety officer.
- Methodical measurement logging and mappingTake measurements using a magnetic induction thickness gauge calibrated against a reference calibration shim. Take at least five measurement points per linear metre of profile, alternating between strategic zones: webs, inner flanges, and outer faces of the profiles.
- Surface preparation for recoatingRemove dust and degrease the surface of the already dried intumescent coat. If the maximum overcoating interval specified by the manufacturer has been exceeded, perform light abrading to ensure mechanical adhesion of the additional coat without compromising the base coat.
- Recoating with intumescent paint and dryingApply the additional quantity required to achieve the exact nominal thickness calculated according to the Ap/V factor. Strictly adhere to substrate temperature (at least 3 °C above the dew point) and ambient relative humidity.
- Validating final thickness and applying the topcoatSystematically carry out re-measurement after through-drying of the additional coat. Apply the protective topcoat against moisture or chemical attack only after definitive validation of the intumescent thickness measurement.
The as-built documentation submitted to site supervision and the cantonal fire protection authorities relies on the final application inspection report. This official document records the exhaustive list of each steel framework component, its calculated section factor Ap/V in inverse metres, the fire resistance rating required by the fire safety concept, the certified intumescent product applied, as well as the complete log of dry film thicknesses recorded after drying. The steelwork contractor certifies by signature that all profiles comply with the requirements of standard SIA 263/1 and the directives of the Association of Cantonal Fire Insurers (AEAI).
Frequently asked questions
How is the Ap/V value of a steel profile determined for intumescent paint?
The section factor Ap/V represents the ratio between the steel surface area exposed to fire (Ap) and the volume of the profile (V). The higher this ratio expressed in m⁻¹, the faster the profile heats up in a fire. The steel contractor extracts Ap/V values from standard profile tables or calculates them based on the number of exposed sides (exposure on 3 or 4 sides) to determine the required thickness from the manufacturer's tables.
Can intumescent paint be applied to achieve an R120 rating on all profiles?
No, the technical feasibility of an R120 classification depends directly on the section factor of the profile. Very slender profiles with a very high Ap/V value cannot generally be protected for a duration of 120 minutes using intumescent paint, because the required dry film thickness would exceed the product's mechanical retention limit on soffits. In such cases, the steel profile must be thickened or alternative solutions such as encasement or spray-applied fireproofing must be used.
What environmental conditions are required for application on the construction site?
Application requires ambient and substrate temperatures above +5 °C (ideally between +10 °C and +30 °C) and a relative humidity below 80 or 85% depending on technical data sheets. Steel temperature must imperatively exceed the dew point by at least 3 °C to prevent any condensation beneath the paint film, which would otherwise impair drying and cause blistering or detachment of the system.
Why must the finishing coat (topcoat) not be too thick?
The finishing coat serves solely to protect moisture-sensitive intumescent paint and provide the desired aesthetic colour. If the topcoat is applied in excessive thickness, it risks restricting the physical expansion of the intumescent paint as temperatures rise during a fire, thereby reducing the effectiveness of the insulating carbonaceous barrier and degrading the guaranteed fire resistance rating.
Texts and standards cited
- SIA 263/1Steel construction - Supplementary specifications
- SIA 118General conditions for construction work