Key takeaways
- Position vent and drainage holes in opposition at the absolute extremities of sections.
- Size openings to a minimum diameter of 10 mm to prevent the box section from exploding.
- Limit asymmetrical assemblies and control plate thickness to prevent thermal buckling.
- Anticipate zinc coating build-up on threads and precision bores before immersion.
Design of degassing perforations, drainage and sizing according to the kettle
Immersing a hermetically sealed hollow body into a bath of molten zinc at 450 °C causes an immediate pressure increase of the trapped air and moisture. Without an escape route, internal overpressure leads to a violent explosion of the workpiece, directly endangering galvanising plant personnel. To guarantee complete immersion without air pockets and smooth drainage of pickling acid and then liquid zinc, every box section, tube or built-up section must incorporate vent and drainage holes.
Holes must be arranged at opposite ends of the workpiece, at the highest and lowest points relative to the dipping angle (generally suspended between 30° and 45°). The size of the openings depends directly on the internal volume of the workpiece. As a general rule, the combined cross-sectional area of the vent and drainage holes must represent at least 7 % to 10 % of the cross-sectional area of the hollow section, with an absolute minimum diameter of 10 mm to prevent rapid blockage by frozen zinc.
| Section dimensions (mm) | Min. degassing diameter (mm) | Min. drainage diameter (mm) | Required positioning |
|---|---|---|---|
| Up to 50 x 50 | 10 | 10 | At extremities, 180° opposite |
| 100 x 100 | 16 | 16 | At dead corners and on end plates |
| 200 x 200 | 25 | 25 | Opposite diagonal and cut-outs |
| Box sections > 300 x 300 | 10 % of cross-section | 10 % of cross-section | Distributed on gussets and stiffeners |
The steel fabricator must ensure that the prefabricated element fits within the usable envelope of the galvanising bath. In Switzerland, standard kettle dimensions range from 7 m to 16 m in length, with depths of 2 m to 3 m and widths of 1.5 m to 2 m. If the workpiece exceeds the bath size, double dipping is required. This imposes an overlap zone in the centre, which creates visual coating build-up and requires additional suspension points on the structure.
Anticipating thermal distortion and post-treatment rework
The sudden rise in temperature during immersion induces massive thermal stresses. Workpieces with asymmetrical shapes, significant thickness variations between assembled elements (for example a thin 3 mm plate welded to a 25 mm base plate), or high levels of residual welding stresses undergo critical buckling. To minimise distortion in thin parts or welded built-up girders, the design must promote a symmetrical distribution of material and welds.
- Symmetrical geometric designAvoid hybrid assemblies of very thin and very thick plates. Use hollowed stiffeners at corners to balance heating.
- Welding stress reliefApply a balanced welding sequence (backstep welding) to reduce internal stresses before dipping.
- Visual inspection and hot or press straighteningImmediately upon removal from the bath, check deflections. Perform re-straightening in a press or by targeted flame straightening on distorted areas.
- Mechanical reworking of holes and threadsRe-tap tapped holes after galvanising or provide initial thread oversizing of 0.4 mm to 0.5 mm.
After the bath, the pure zinc and iron-zinc alloy layer creates an extra thickness of 80 to 150 microns depending on the section and the silicon content of the steel (Sandelin effect). This layer obstructs assembly holes and accumulates zinc runs or teardrops at the bottom of workpieces. Contact surfaces for high-strength (HS) bolts require specific preparation by light grinding or mechanical wire brushing to guarantee the design slip factor.
The steel fabricator is required to execute fabrication in accordance with professional trade standards. Pursuant to the general principles of the Code of Obligations (CO), the contractor is liable for the proper execution of the works and the conformity of protections applied by its subcontractors. If an assembly exhibits a fitting defect due to unanticipated distortion, rectification and supplementary machining are entirely at the fabricator's expense.
Design of holes and integration with kettle envelopes
Immersing a rolled steel or closed box structure into a bath of molten zinc heated to approximately 450 °C generates an instantaneous pressure increase of trapped air and moisture. Without continuous circulation of the liquid and complete venting of gases, the risk of the hollow section exploding under steam pressure is major, as is the risk of the workpiece floating in the kettle due to buoyancy. The steel fabricator must size and strategically position degassing openings (vents) and zinc drainage holes as early as workshop fabrication drawings are prepared.
As a general rule, the combined cross-sectional area of the vent and drainage holes must represent at least 25 % of the cross-sectional area of the hollow section or assembled hollow body. To ensure smooth filling and complete emptying without residues during slinging of the workpiece at approximately 45° in the kettle, minimum hole diameters must be scrupulously implemented by fabricators.
| Hollow section size (mm) | Min. diameter per opening (mm) | Number of openings per end | Mandatory positioning |
|---|---|---|---|
| Tube ≤ 50 x 50 | 10 | 1 drain / 1 vent | Diagonally opposite edges |
| Tube 60 x 60 to 100 x 100 | 16 | 1 drain / 1 vent | Diagonally opposite edges |
| Section 120 x 120 to 200 x 200 | 20 to 25 | 2 drain / 2 vent | At 4 corners of end plate |
| Box section > 200 x 200 | 30 to 50 | Multiple (depending on volume) | At high and low slinging points |
The overall geometric sizing of the assembled element must be rigorously checked against the usable capacity of the galvanising tank at the treatment facility. If a workpiece exceeds the dimensions of a standard Romand tank (generally between 7 and 16 metres in length, 1.5 to 2 metres in width, and 2.5 to 3 metres in depth), double dipping (successive dipping by turning the piece) becomes unavoidable. This operation doubles the thermal loading on the central sub-assembly and increases the risk of zinc build-up along the overlap line.
Thermal distortion, pickling and interface finishing
Immersion into a bath at 450 °C instantly releases internal mechanical stresses introduced during rolling, plasma cutting or welding of sections. Asymmetrical parts, assemblies combining large thickness differences (for example a 3 mm plate welded to a solid 15 mm section) or large thin-plate surfaces are particularly susceptible to buckling, localised crippling and permanent warping.
- Preventive design in the engineering officeGive priority to symmetrical sections, balance weld positions relative to the neutral axis, and apply uniform wall thicknesses. Avoid locked pre-assemblies that prevent free expansion during the temperature rise.
- Preparation of welded assembliesProduce stitch or bevelled welds without trapping weld slag. Thoroughly descaling and avoid non-pyrolysable marking paints prior to shipment to the galvaniser.
- Post-treatment inspection and straighteningCarry out systematic dimensional checks upon receipt. Straightening is carried out either on a cold hydraulic press under controlled force, or with an oxy-fuel torch by controlled flame straightening without exceeding the degradation temperature of the iron-zinc alloy layer.
Post-galvanising finishing operations are essential to guarantee assembly and structural accuracy on the construction site. Because molten zinc fills voids, tapped threads must imperatively be re-chased after treatment, or else oversized during fabrication in accordance with metric thread tolerance standards for galvanising. Bearing surfaces intended for fitted high-strength bolted connections must be cleared of zinc runs and drips by light grinding or precise scraping to ensure the calculated slip factor.
If the steel fabricator finds that the material selection or engineering provided by the construction management exposes the work to unavoidable distortion or the impossibility of proper drainage, it shall immediately inform the client in accordance with art. 365 CO al. 3 in order to demand the necessary design modifications.
Managing non-conformities, bath explosions and post-galvanising repairs
Immersing a hollow section or sealed box section into a molten zinc bath at approximately 450 °C causes instantaneous flashing of trapped ambient air and moisture. In the absence of a vent hole to balance pressures, internal overpressure causes an explosion in the bath, projecting molten zinc and destroying the workpiece. When a steel sub-assembly is rejected or distorted upon exit from the galvanising plant, the site supervisor and the workshop manager must immediately apply an emergency procedure to secure production and address the failure.
- Securing the area and visual inspectionIn the event of a dipping incident, isolate the affected batch. Inspect the galvanised part to identify cracks at welds, excessive deflections caused by the relaxation of thermal stresses, and the condition of the vent holes.
- Mechanical reworking and straighteningStraightening of thin parts or hot-deformed sections is performed using a cold press or by controlled flame straightening. If machining or grinding is required on contact surfaces or assembly holes, the original protective layer is destroyed.
- Restoring corrosion protectionAny ground, post-drilled or straightened area must undergo degreasing, mechanical wire brushing (thorough grade of preparation) and the application of a zinc-rich paint (Zinc-Rich Primer) or a thermal-sprayed zinc alloy coating (metallising), in accordance with steel construction trade standards.
If the defect arises from a discrepancy between workshop design and the geometry of the galvaniser's kettles (incompatible bath dimensions imposing an unanticipated double dip), the steel fabricator must enforce contractual liability in accordance with the provisions of the Code of Obligations (CO) governing contracts for work and services (art. 364 CO). In the event of non-conforming delivery or parts distorted beyond structural erection tolerances, the client may exercise its rights regarding defects pursuant to CO to demand rectification of the elements.
Frequently asked questions
Why does a closed steel component explode in the galvanising bath?
During immersion in molten zinc at 450 °C, air and moisture trapped in an unvented hollow section undergo extreme thermal expansion. Internal pressure rises instantaneously until it exceeds the ultimate strength of the steel or welds, causing violent tearing of the section and hazardous projections of molten zinc.
How are vent and drainage holes sized on a steel box section?
Vent holes (at the high end during dipping) and drainage holes (at the low end) must have a minimum cross-sectional area equivalent to at least 25 % of the internal cross-section of the section for small tubes, and at least 50 mm in diameter for large volumes. They must be placed at opposite ends to avoid any air or acid pockets.
How is thermal distortion of a thin part corrected after galvanising?
Thin plates and asymmetrical structures distort under the effect of thermal stresses from the bath. Straightening is carried out in the workshop using a hydraulic press or by targeted flame straightening with a torch. If the galvanised coating is damaged during heating or mechanical work, it must be restored immediately.
What are the solutions for repairing galvanising after rework on the construction site?
On areas cut, drilled or ground after treatment, the steel must be cleaned to bare metal by brushing or light grinding, and then coated with a high-solids zinc-rich paint (at least 90 % zinc in the dry film) or repaired by thermal spraying of a zinc-aluminium wire.
Texts and standards cited
- CO art. 364obligations of the contractor: liability subject to the same rules as that of an employee; the contractor executes the work in person or under personal direction; unless otherwise customary or agreed, the contractor provides the necessary means, equipment and tools at its own expense.
- COrights of the client in the event of defects in the work: rejection, price reduction, rectification, damages; any clause agreed upon in advance that limits or excludes the right to rectification of defects is void if the defect relates to an immovable structure (al. 2bis, since 1 January 2026).