Key takeaways
- An expired welder qualification certificate makes the joint non-compliant under standard SN EN 1090.
- The welding procedure specification strictly dictates electrical parameters and filler metals.
- Six-monthly prolongation of the certificate by the employer conditions the two-year validity issued by the certifying body.
- The inspector checks on site the exact match between the assembled component, the certificate, and the WPS.
Mandatory supporting documents before the first arc strike
On a structural steel construction site subject to standard SN EN 1090, executing a weld bead without a prior technical file constitutes a major manufacturing defect. Switching on the welding set requires two inseparable contractual documents: the welder qualification certificate and the welding procedure specification, commonly designated by the abbreviation WPS (DMOS). The absence of these supporting documents during an inspection by site management or the civil engineer leads to the immediate rejection of the framing elements concerned, regardless of the visual quality of the weld bead.
- Welding Procedure Specification (WPS / DMOS)
- Workshop or erection document recording the operating parameter ranges required to ensure the repeatability and mechanical strength of a given joint: steel grades, type of shielding gas, wire or electrode diameter, current, voltage, wire feed speed, preheat temperature, and pass sequences.
The erection manager or site foreman must have certified copies of these documents on the structure. The WPS reflects the requirements of the execution file and is based on a welding procedure qualification validated beforehand. The welder does not choose parameters by guesswork; they set their power source according to the range defined on their work sheet. Under art. 364 CO, the contractor is liable for the proper execution of the entrusted work, which implies using the appropriate technical resources and maintaining documentary control of the processes.
| Operating element | Standard technical requirement | On-site verification |
|---|---|---|
| Welding process | Arc welding with flux-cored wire or solid wire under gas shield | Inspection of torch, wire feeder, and active gas mixture cylinder |
| Filler metal | Solid wire or covered electrode matching the parent metal grade (S235, S355) | Check of 3.1 material certificates and designation on packaging |
| Current and voltage range | Bounded range in amperes and volts according to thickness of flanges and webs | Reading of digital displays on the welding unit during the filling pass |
| Interpass temperature | Maintaining a minimum preheat threshold and limiting maximum heat | Measurement using a contact thermometer or tempil stick on parts |
Range of approval, tracking over time, and joint inspection on site
A welder qualification certificate does not confer universal clearance. Each certificate defines a strict field of activity: welding process, joint type (butt weld or fillet weld), material group, thickness range, pipe diameters if applicable, and welding position (flat, vertical-up, horizontal, or overhead). If an erector holding a flat qualification performs a vertical-up weld on a portal frame node, the component is declared non-compliant under standard SN EN 1090, requiring full rework or additional non-destructive testing.
- Visual check of identity documents and certificatesThe foreman checks the worker's name on site against the original document or the official copy of the qualification test issued by the approved body.
- Examination of expiry date and periodic signaturesVerification of overall certificate validity and checking of the employer's six-monthly sign-offs confirming continuous practice of the process.
- Cross-referencing the field of application with the erection planValidation of the assembly position required on the structural node against the reference letters appearing on the erector's qualification.
- Displaying the WPS at the workstationPhysical provision of the laminated procedure sheet right at the welding area for direct consultation by the welder and inspectors.
Practising the trade requires absolute documentary rigour to ensure the structural safety of buildings. In the event of a serious failure to observe the recognised rules of the trade in managing or executing work endangering third-party safety, art. 229 CP establishes the criminal framework penalising offences committed intentionally or through negligence. The traceability file, including the WPS sheet, valid staff certificates, and non-destructive testing reports, forms legal proof of the compliance of the delivered steel structure.
Strict match between WPS and certificate: parameters to lock down
On a structural steel construction site subject to standard SN EN 1090, the welding set may only be turned on after cross-checking the ranges of approval. The welding procedure specification sets execution limits for each frame joint. The welder qualification certificate must cover all of these operational variables. A deviation in a single essential variable renders the joint non-compliant in the eyes of site management and the welding coordinator.
| Execution variable | Parameter required by the WPS | Coverage required on the certificate |
|---|---|---|
| Welding process | Process 111 (covered electrode) or 135 (solid wire MAG) | Process number strictly identical to the selected welding procedure |
| Joint type and geometry | Butt weld (BW) with back gouging or backing strip | BW qualification covering fillet welds (FW) under the standard |
| Parent metal group | Structural steel S235, S275, or S355 | Equal or higher grade group (matching filler metal) |
| Material thickness (t) | Actual thicknesses of flanges, webs, and gusset plates in millimetres | Qualified thickness range encompassing the value of the joint to be welded |
| Welding position | Vertical-up (PF), flat (PA), or overhead (PE) position | Test positions formally authorising the orientation of the weld bead |
Adjusting electrical parameters is the second critical point. Current, arc voltage, and travel speed must remain within the heat input ranges prescribed by the WPS. Poorly controlled heat input alters the toughness of the steel in the heat-affected zone. The site foreman ensures that the welder has a laminated WPS sheet attached directly to the welding power source.
Joint audit on site and handling of documentary non-conformities
Supervision of jointing work requires flawless traceability. During an unannounced inspection by the engineer or specialist consultant, the workshop and erection file must be immediately available for review. This file includes the welder qualification certificate with its six-monthly sign-offs, the approved welding procedure specification, and the associated procedure qualification record. The absence of these documents during inspection leads site management to stop the welding set.
The temporal validity of the certificate relies on dual confirmation. Every six months, the welding coordinator or the employer confirms in writing that the worker has continuously worked within their range of qualification, without an interruption exceeding six months. Full renewal of the practical test occurs at the expiry date set by the applicable technical regulations, generally every two or three years depending on the chosen qualification route.
- 1. Prior check before arc strikeCheck the welder's stamp, the date of the last six-monthly sign-off on the certificate, and the exact match between the joint to be welded and the WPS displayed at the station.
- 2. Marking the completed beadHave the individual welder identification stamp applied using an indelible marker or cold stamping in the immediate vicinity of each completed pass.
- 3. Non-destructive testing and sign-offHave 100% visual inspection carried out and record any dye penetrant, magnetic particle, or ultrasonic testing prescribed according to the execution class of the frame.
- 4. Recording in the erection reportFile daily inspection sheets in the construction site quality assurance folder for submission to the client.
On-site organisation precludes any improvisation. If a joint modification arises during erection, the installation manager must immediately refer it to the project engineer or technical design office before adapting the WPS. The involvement of an external expert commissioned to assess defective joints represents rework costs of several thousand francs, not to mention lifting delays that halt overall progress of the structural work.
Crisis management on site: missing documents and stoppage of welding
When a civil engineer or site management orders a halt to welded joints during erection, the cause is almost systematically a documentary failure: an expired welder qualification certificate, a welding procedure specification (WPS) missing from the construction site folder, or a mismatch between the executed process and the qualification held. In structural steelwork subject to standard SN EN 1090, any weld performed without valid documentary cover automatically loses its presumption of conformity. The structure can then no longer be accepted as it stands.
- Immediate quarantine of the welded jointThe site supervisor stops the welding set, marks the bead with industrial paint marker, and quarantines the assembled elements (sections, gusset plates, or base plates). No cosmetic grinding is tolerated. The welding log records the erector's identity, the actual measured parameters, and the exact location on the erection drawings.
- Technical assessment with the welding coordinatorThe company's welding coordinator intervenes to benchmark the case against standard SN EN 1090. If the welder possessed the practical skills but lacked the six-monthly prolongation signature, 100% non-destructive testing (penetrant testing, magnetic particle testing, or ultrasonic testing) is ordered to determine the internal soundess of the weld bead.
- Removal and rework according to compliant WPSIf the certificate proves completely unsuitable for the material group, welding position, or thickness, the bead is deemed void. Art. 366 CO provides that if the work is executed defectively or contrary to the contract through the fault of the contractor, the client may set a reasonable deadline for rectification. The joint is then entirely gouged by air-arc or ground out, then rebuilt by a qualified welder under a validated WPS.
Frequently asked questions
The six-monthly signature on a welder certificate is missing: can we weld?
No. Under standard SN EN 1090, a welder qualification certificate without the employer's six-monthly signature confirming continuous practice has lapsed. The operator may not execute any load-bearing joint. The welding coordinator must check the pieces produced over the last six months and have the qualification prolonged by the certifying body before any new arc strike on the construction site.
Can a workshop WPS be applied as is to outdoor erection?
No. Swiss construction site conditions require adapting the welding procedure specification to climatic and geometrical constraints. An erection WPS incorporates steel preheating in low temperatures, draught shielding to protect the molten pool under shielding gas, and actual welding positions at height, which are often more restrictive.
What does the contractor risk if a joint is welded outside the range of approval?
Site management refuses acceptance of the structural node. Since the element is not covered by standard SN EN 1090, the engineer may demand exhaustive non-destructive testing at the steel fabricator's expense, or even total removal of the weld bead by gouging. In the event of a prolonged dispute, the client may commission a third party to redo the joint at the defaulting company's expense.
Who is authorised to draft and validate the WPS on the construction site?
The welding procedure specification must be drawn up by the welding coordinator of the workshop or technical design office, based on a recorded welding procedure qualification test. The erection supervisor or site foreman scrupulously applies the sheet on site (current, voltage, filler metal), but does not have the technical authority to modify its execution parameters arbitrarily.
Texts and standards cited
- SN EN 1090Execution of steel structures and aluminium structures
- COdelay and predictably defective execution
- CP art. 229breach of the recognised rules of the art of construction