🧱 CFC 215Corrosion protection and fire resistanceChapter 5 of 10 in the section

Galvanic corrosion: steel, stainless steel and aluminium in contact, and the required insulation

This chapter deals with electrochemical mechanisms applicable to mixed connections in metal construction. You will learn to assess the risk of galvanic couples depending on the materials present, to design the Electrical Break using synthetic insulators, and to secure fixings subjected to external moisture.

Key takeaways

  • The simultaneous presence of dissimilar metals and water creates a destructive galvanic cell.
  • The electrical potential difference determines the severity of corrosion on the anodic metal.
  • An unfavourable surface area ratio dramatically accelerates the rate of attack on the less noble metal.
  • Systematic insulation using a sealing sleeve and polymer washer prevents premature failure of fixings.

Mechanism of the galvanic couple and influence of the potential difference

In metal construction, direct contact between two different metals in the presence of an electrolyte (rainwater, condensation or saline moisture) creates an electrochemical cell. The less noble metal (the anode) undergoes accelerated dissolution to the benefit of the more noble metal (the cathode). This phenomenon, known as galvanic corrosion, directly affects the durability of facade frameworks and load-bearing substructures.

Standard dissolution potential
A value expressed in volts measuring the nobility of a metal in a given medium. The higher the potential difference between two metals in contact, the more intense the galvanic current and the faster the corrosion.
Coupling behaviour between common metals in mixed facades
Metal combinationIndicative potential differenceRisk levelMandatory design measure
Aluminium / Stainless steel A2-A4Low to moderate (~0.15 V)Low if correct surface area ratioEPDM sealing washer recommended outdoors
Aluminium / Galvanised steelModerate (~0.25 V)Medium in damp environmentsElectrical insulation of interfaces or powder coating
Aluminium / Bare carbon steelHigh (~0.50 V)Very highDirect contact prohibited, full insulation required
Galvanised steel / Stainless steel A4High (~0.45 V)HighMechanical separation and bolt sleeving

Besides the nature of the metals, the relative surface area of the anode and cathode plays a decisive role in the rate of degradation. A small anode in contact with a large cathode (for instance a zinc-plated steel screw fixed to a large stainless steel sheet) undergoes extremely violent attack, leading to rapid failure of the fixing. Conversely, a large anode (aluminium structure) combined with a small cathode (stainless steel screw) exhibits a very low current density and distributed, virtually harmless corrosion.

Insulation devices and fixing details in load-bearing facades

In the field of mixed facades with a load-bearing metal structure, prevention relies on the physical interruption of electrical continuity. If water cannot be completely eliminated from the construction detail, an unalterable dielectric component must be inserted between the incompatible metal surfaces.

  1. Placing the insulating bush (insulating sleeve)To avoid any axial contact between the shank of the threaded bolt and the hole in the aluminium section, insert a flanged bush made of polyamide (PA66) or PTFE inside the hole.
  2. Fitting elastomeric backing washersPlace large EPDM or polypropylene washers under the screw head and under the nut to prevent direct surface contact between the bearing flange and the structure.
  3. Interposing an isolating stripApply a neoprene strip or an extruded insulation profile to the bearing surface of powder-coated steel facade brackets supporting secondary aluminium framework components.
  4. Torque-controlled tighteningApply the specified tightening torque without crushing the insulating washer, otherwise the polymer component may be destroyed and direct metallic contact restored.

During assembly on the construction site, the metal constructor systematically checks compliance with the protective assemblies specified on the detailed working drawings. If the main anchoring substrate provided by another trade exhibits non-conformities or plumb deviations requiring unforeseen shimming, the constructor's duty to notify and reporting requirements are governed by the general framework of the Code of Obligations (CO).

Cathodic and anodic surface area ratio and corrosion kinetics

Galvanic corrosion does not depend solely on the anodic potential difference between two metals in the presence of an electrolyte such as condensation or runoff water. The decisive parameter for the rate of degradation lies in the relative surface area ratio between the more noble metal (the cathode) and the less noble metal (the anode). When a small anodic surface area is coupled with a large cathodic surface area, the corrosion current density concentrates entirely on the less noble metal, leading to extremely rapid perforation or loss of structural cross-section.

In load-bearing metal construction, the classic case of a galvanised steel screw securing a large stainless steel plate illustrates this destructive phenomenon: the stainless steel captures electrons over its entire surface while the zinc and then the steel of the screw dissolve within a few months. Conversely, using stainless steel fixings on aluminium or galvanised steel frameworks or claddings offers a very favourable surface area ratio. As the anode (the structure or panel) is much larger than the cathode (the screw head), the current density is diluted and corrosion remains negligible, provided that trapped stagnant moisture is controlled.

Galvanic behaviour of bimetallic connections in exposed facades
Connection (Anode / Cathode)Typical surface area ratioGalvanic risk levelRequired insulation measure
Galvanised steel screw on A2/A4 stainless steel plateHighly unfavourable (small anode / large cathode)Critical (rapid corrosion of the fixing)Prohibited: replace with insulated stainless steel fixing
Aluminium bracket on carbon steel structureVariable depending on nodeHigh in damp environmentsEPDM or polyamide thermal/dielectric break + sleeve
A4 stainless steel fixing on anodised aluminium frameHighly favourable (small cathode / large anode)Low to moderateEPDM washer under head to prevent local attack
Untreated steel bolting on stainless steel bracketUnfavourable (small anode / large cathode)Very highFull insulation of the bolt body and washers

Installation of galvanic breaks and facade fixing details

To permanently break the electrical circuit in a mixed facade connection, inserting a simple flat washer under the screw head or nut is not sufficient. Direct metallic contact also occurs along the shank of the bolt or anchor stud as it passes through the clearance holes of the parts being joined. An effective galvanic break requires the combined use of a flanged insulating sleeve (or shouldered bush) made of polyamide or POM, extending entirely through the penetrated component, and thick synthetic washers under both head and nut.

In heavy load-bearing metal facade fixing details, shear and compression forces must be carefully analysed when selecting insulating materials. EPDM or neoprene spacers are ideal for sealing and insulation under moderate loads, but they risk creeping under high concentrated loads. For bracket bases or bracing connections, insulating plates and bushes made of glass-fibre reinforced polyamide or reinforced epoxy resin are preferred, as they can transmit mechanical loads without crushing while guaranteeing high electrical resistance.

  1. Hole preparationDimension the hole diameter in the anodic part taking into account the thickness of the insulating sleeve barrel (generally add 2 to 3 mm to the nominal shank diameter).
  2. Positioning the isolating spacerFit the rot-proof insulation plate (polyamide, hard EPDM) over the entire contact area between the aluminium element and the structural steel.
  3. Inserting the flanged sleeveSlide the insulating sleeve into the hole to completely line the through-hole and prevent any radial contact with the bolt shank.
  4. Controlled tighteningPlace the stainless steel washer onto the synthetic insulating washer, then tighten to the specified torque without excessively crushing the polymer component.

In case of doubt regarding the compatibility of the materials specified by the design office or the risk of water pooling at an anchoring detail, the metal constructor applies their duty to notify under the Code of Obligations (CO). Watertightness of the connection node is an inseparable complement to electrical insulation: in the absence of water or condensed moisture acting as an electrolyte, the electrochemical reaction cannot be initiated.

Management of galvanic defects and corrective actions on facades

On a metal construction or mixed facade construction site, late detection of galvanic corrosion usually manifests as visible rust stains beneath fixing points, blistering of the aluminium powder coating, or severe bolt seizing. This phenomenon appears as soon as an electrolyte (rainwater, condensation retained by capillary action, salt spray) bridges two metals with different potentials, such as an aluminium framework bracket bolted directly onto a galvanised carbon steel strut without an electrochemical break.

  1. Diagnosis and visual inspection of the connectionInspect the condition of the facade connections. Measure the loss of section on the anode metal (typically the galvanising zinc or the aluminium) and check whether the facade's watertightness is compromised.
  2. Disassembly and neutralisation of oxidesRemove failed fixings. Mechanically treat corroded surfaces, eliminate aluminium oxide or iron hydroxide powders, then apply a protective primer compatible with the substrate.
  3. Reinstatement of the galvanic breakInterpose an insulating shim made of structured elastomer (EPDM) or high-density polymer between the dissimilar metal parts. The shim must project at least 2 mm beyond the outline of the more noble profile.
  4. Replacement of bolting with shank insulationInsert a polyamide or POM insulating bush into the hole to prevent any contact between the bolt shank and the hole wall. Add plastic insulating washers under both head and nut.

From a legal and contractual standpoint, liability for remedial work due to defective galvanic insulation falls under the warranty for defects regime under art. 368 CO. The client has a limitation period of five years under art. 371 CO to assert their rights regarding elements incorporated into the immovable work. The metal constructor must ensure that the facade system data sheets explicitly specify galvanic breaks prior to any implementation on the construction site.

Frequently asked questions

Can aluminium brackets be fixed directly to a stainless steel structure?

Direct assembly presents a risk of aluminium corrosion if condensation stagnates. As stainless steel is more noble, the unfavourable surface area ratio accelerates the degradation of the aluminium. A synthetic shim made of EPDM or polyamide must be interposed, and insulating sleeves must be used on the anchor screws.

How can crushing of insulating washers be prevented when tightening bolts?

Tightening must be controlled using a torque screwdriver or torque wrench according to the manufacturer's recommendations. The use of reinforced insulating washers or hard polyamide bushes prevents material creep under pressure while maintaining the vital electrical break between the bolt head and the metal part.

Does hot-dip galvanised steel react when in contact with aluminium in a mixed facade?

In dry conditions, the risk remains low. In an outdoor damp or urban atmosphere, however, the zinc is consumed to protect the steel, and the aluminium then undergoes pitting corrosion in contact with the exposed steel. Elastomeric insulation is still required between the aluminium profile and the galvanised steel support.

What is the difference between a simple washer and an insulating sleeve?

An insulating washer only isolates the bearing surface under the head or nut. An insulating sleeve has a cylindrical barrel that penetrates into the hole of the profile. It prevents direct contact between the threaded shank of the fixing and the inside of the clearance hole in the assembled component.

Texts and standards cited

  • Code des obligations art. art. 368 CORights of the client in case of defects in the work (price reduction, remediation, damages).
  • Code des obligations art. art. 371 COLimitation period for the client's rights arising from defects in an immovable work (five years).

In the same section