Key takeaways
- The use of anchors with cracked concrete approval is mandatory under dynamic loading.
- Meticulous blowing and brushing of the borehole directly govern the mechanical strength of the anchor.
- Compliance with center-to-center spacings and edge distances prevents failure by concrete breakout.
- The on-site pull-out test validates the effective load-bearing capacity of the anchor under proof load.
Anchor selection and geometry in cracked concrete
The connection between the steel structure and the reinforced concrete infrastructure constitutes the most heavily stressed load-transfer zone of the structure. In the tension zone of reinforced concrete elements, the formation of bending or shrinkage cracks is inevitable. The steel constructor must imperatively use mechanical expansion anchors or chemical anchors with a valid European Technical Assessment for cracked concrete. An anchor not certified for cracked concrete risks slipping or losing its expansion as soon as a through microcrack appears at the drilled hole.
- Cracked concrete (tension zone)
- Zone of the reinforced concrete structure where tensile stresses exceed the tensile strength of the concrete, creating microcracks in which the anchor must maintain its load capacity.
The geometric design of the anchor base plate requires strict compliance with the effective embedment depth, center-to-center spacing between studs, and distances to the free edges of the member. If an anchor is installed too close to a corner or slab edge, the expansion force or the concrete breakout cone causes spalling of the concrete edge. Manufacturers' technical data sheets specify these absolute limit values, which must be adapted according to the thickness of the fixture to be secured.
Borehole preparation and execution of on-site tensile tests
The primary cause of premature failure in chemical or mechanical anchors lies in the presence of drilling dust accumulated at the bottom of the hole. Drill cuttings create an insulating layer that prevents resin adhesion or reduces friction of the expansion sleeve. The cleaning procedure must systematically alternate mechanical and pneumatic dedusting phases.
- Drilling to the specified diameterDrill the hole perpendicularly to the concrete surface using a compliant drill bit, respecting the required embedment depth plus systematic over-drilling.
- Pneumatic blowingInject oil-free compressed air into the bottom of the borehole using an extended nozzle to blow out coarse dust.
- Mechanical brushingRun a wire brush of a diameter matching the hole with a back-and-forth motion to dislodge dust caked on the walls.
- Final dedustingRepeat air blowing until all particulate residues are fully expelled.
To validate anchor compliance and substrate quality in accordance with site safety directives, direct pull-out verification tests are performed on a sample of anchors. The test consists of applying an axial proof load using a hollow hydraulic cylinder fitted with a calibrated pressure gauge. This procedure verifies anchor behaviour without reaching failure of the connection. If the strength of the host concrete is non-compliant, the provisions set out in the Code of Obligations (CO) apply regarding the notice of defects.
Work is planned such that the risk of occupational accidents, occupational illnesses, or damage to health is kept as low as possible.
art. 3 OTConst
Drilling execution and rigorous dedusting protocol
Fastening a structural steel base plate to a reinforced concrete substrate represents one of the most critical interfaces on the construction site. The theoretical load-bearing capacity calculated by the engineer is only valid if load transfer occurs in sound material and according to a rigorously observed installation protocol. In cracked concrete, subjected to dynamic loading or combined tension and shear stresses, anchor performance directly depends on cavity condition at the moment of setting or injection.
- Drilling to specified dimensionsDrill using a rotary hammer drill fitted with a four-cutter carbide bit to ensure hole roundness. Scrupulously adhere to the minimum effective embedment depth h_ef and diameter specified by the manufacturer. If passive rebar is encountered, never cut the reinforcement without prior approval from the structural engineer.
- Alternating blowing and brushing (2x2 or 4x4 rule)Clean the cavity according to the approval protocol: blow out the bottom of the hole using a manual blow-out pump or oil-free compressed air, brush the walls with a wire brush matching the drill bit diameter, then blow out again. Repeat this sequence at least twice to eliminate all adhering fine particles.
- Visual inspection and depth measurementCheck internal cleanliness with an inspection torch and measure the effective hole depth with a depth gauge. Drilling depth must exceed anchor rod embedment depth to accommodate any remaining debris and prevent anchor jamming.
Tensile testing procedures and on-site validation
Once base plates are positioned and anchors torqued to the specified torque using a torque wrench, direct pull-out verification tests may be required by the site management or the engineering office. These on-site tests validate concrete substrate compliance, adherence to the cleaning procedure, and the absence of slippage under service load or design load.
| Type of inspection | Required equipment | Applied force | Validation criterion |
|---|---|---|---|
| Non-destructive torque check | Calibrated torque wrench | Nominal installation torque (T_inst) | No unwanted rod rotation, target value reached without yield/creep |
| Proof load pull-out test | Hollow hydraulic cylinder with pressure gauge | 1.2 to 1.5 times the recommended service load | Load sustained for 2 minutes without measurable stud displacement |
| Destructive test on sacrificial anchor | Tensile tester with displacement sensor | Load up to failure of concrete or steel | Failure mode matching ETA data sheet expectations (pull-out, concrete cone, steel) |
Erection work must be carried out in compliance with professional trade standards and site scheduling. For all steel structure and load-bearing facade erection activities, worker safety and the provision of fall protection measures remain governed by the Construction Works Ordinance (OTConst).
Management of non-conformities and tolerance exceedances
When an on-site pull-out or tensile test reveals premature slippage, anchor sleeve pull-out, concrete cone failure, or an inability to reach the proof load specified by the engineering office, the site foreman must immediately order a halt to base plate installation in that area. Non-conformity of a mechanical or chemical anchor in concrete generally stems from overestimating actual substrate quality, undetected dense rebar hindering expansion, or insufficient borehole cleaning. The steel construction company must under no circumstances over-torque to compensate for insufficient holding power.
- 1. Drawing up the non-conformity reportAccurately record obtained failure or slippage loads, geometric locations of defective anchors, and concrete substrate behaviour in the site logbook.
- 2. Joint analysis with the civil engineerForward the test report to the engineering office. Only the structural engineer can recalculate the connection and authorise a remedial solution such as resizing the anchor base plate.
- 3. Installing replacement anchoringDrill new holes observing minimum edge distances and center-to-center spacings, or opt for high-performance chemical anchors after full remediation of the area.
In the event of flagrant disregard of the accepted rules of technology endangering structural stability or human safety, art. 229 CP provides for criminal sanctions against the installers. Rigorous maintenance of technical approval sheets, the torque wrench calibration log, and pull-out test reports guarantees full traceability of the interface between structural work and the steel structure.
Frequently asked questions
What should be done if the anchor spins freely during torque tightening?
When a mechanical anchor spins without reaching the specified torque, the expansion mechanism has failed to grip the concrete. This often indicates an oversized hole, crumbly concrete, or a void. The component must be dismantled, the failed anchor removed or cut flush, and the fixing point relocated. If relocating is impossible, using an injected chemical anchor after strict cleaning is required, subject to engineer approval.
Is it permitted to enlarge a base plate hole on site if the drilled hole is misaligned?
Misalignment of holes in concrete relative to the steel base plate is a classic construction site occurrence. Slotting a hole using an angle grinder or cutting torch is prohibited without prior approval. It reduces the washer bearing surface and impairs shear resistance. The compliant solution consists of using thick welded load-spreading washers or adjusting the anchor position within permissible tolerance limits.
How should one react if rebar is severed while drilling for the anchor?
Severing a rebar in reinforced concrete can compromise the load-bearing capacity of the structure. If rebar is struck, drilling must stop immediately. The steel constructor must inform the site management and the civil engineer. If the rebar cannot be cut, the hole must be abandoned, filled with non-shrink structural repair mortar, and the drilling relocated while complying with standard center-to-center spacings.
Why is a torque wrench mandatory for base plate assembly?
The torque wrench guarantees application of the exact tightening torque specified by the anchor manufacturer. Under-tightening prevents correct cone expansion, reducing pull-out resistance. Over-tightening risks damaging threads, shearing the steel, or causing premature concrete cracking. Only controlled tightening validates fixing compliance and guarantees design load resistance in accordance with the approval.
Texts and standards cited
- CP art. 229violation of the rules of the art of building