Painted floors and resins: substrate moisture: the execution reference
Intended for team leaders and site managers in industrial and building painting, this section deals with decisions on applying resin floor coatings. It sets the admissible moisture thresholds, the calcium carbide test method, the technical limits of epoxy barriers and the rules for mechanical preparation and application. The painter will find here the precise criteria for accepting a substrate or formally refusing to proceed.
- 10chapters
- 22 000words
- 6sections in the training course
- 60chapters in total
Key values to remember 5
4.0 %
Maximum admissible moisture content for cement screed without underfloor heating
2.5 %
Maximum admissible moisture content for cement screed with underfloor heating
0.5 %
Maximum moisture content for heated calcium sulphate anhydrite screed
1.5 N/mm²
Minimum surface cohesion of the concrete substrate before resin application
+3 °C
Minimum required difference between substrate temperature and dew point
Scope of the resin-floor painter and trade boundaries
Applying a synthetic coating or a floor paint falls within the competences of the painter under CFC 272. The painter's role begins with the rigorous assessment of the raw mineral substrate before any mechanical or chemical intervention. The painter's task is neither to design nor to pour the screed, as these services fall to the screed layer (CFC 281). Nor does the painter step in to correct major defects of structural flatness or falls, which must be reported to site management during the initial joint inspection record.
On the construction site, the operational boundary is strict: the painter checks the compatibility of the substrate with the specified resin system. If the ambient thermo-hygrometric conditions, the dew point or the water content of the screed exceed the tolerances of the manufacturers' data sheets and of the applicable standards, the applicator must suspend operations. In accordance with art. 365 CO, the contractor is obliged to notify the client in writing immediately when the substrate supplied shows anomalies that jeopardise the proper performance of the work.
| Site operation | Responsible trade | Reference document |
|---|---|---|
| Acceptance measurement of the screed and drying protocol | Screed layer (CFC 281) | Standard SIA 251 |
| Moisture check before application and dew point | Resin-floor painter (CFC 272) | Standard SIA 257 |
| Mechanical surface preparation (shot blasting, grinding) | Resin-floor painter (CFC 272) | Standard SIA 257 |
| Treatment of structural expansion joints | Civil engineering / Site management | Standard SIA 271 / SIA 118 |
The painter's moisture measurement is not intended to certify the screed in the sense of the screed layer's acceptance of the work, but to validate a reliable application window for the adhesion of epoxy or polyurethane resins. Applying onto a water-saturated substrate inevitably leads to delamination under osmotic pressure, for which the resin applicator will bear full responsibility if he has not recorded his prior measurements.
Sequential intervention protocol: from opening the substrate to handover
To avoid premature debonding, blistering or curing delays, the construction of a resin floor follows an unavoidable chronological technical order. The ten chapters of this section are structured according to this workshop and site logic, guiding the tradesperson from the acceptance check through to the final commissioning verifications.
- Moisture validation and temporary barriersThe first step is to measure the actual water content of the substrate with the carbide device (chapter 1). Where an insurmountable schedule constraint exists, the use of a special epoxy barrier for damp substrates must be assessed with its strict technical limits (chapter 2).
- Mechanical preparation and chemical selectionMechanically opening up the substrate by shot blasting or planing must remove the surface cement laitance (chapter 3). The choice of resin, rigid epoxy or flexible polyurethane, is then determined by the mechanical, thermal and chemical demands of the room (chapter 4).
- Application, joints and perimeter finishingPrecise dosing of the components and management of the pot life ensure that the film cures properly (chapter 5). The resin applicator then treats the contraction joints without restraining them (chapter 6) and forms the rounded coves for watertight skirtings (chapter 7).
- Texturing, drying and handling of claimsIncorporating calibrated quartz fillers provides the required slip-resistance class according to the safety requirements (chapter 8). The waiting times before foot traffic and heavy traffic are resumed must be scrupulously observed (chapter 9), while blistering mechanisms require a methodical diagnosis in the event of a claim (chapter 10).
📘 Chapters in this section 10
The figure that decides: screed moisture, measurement method and threshold by binder
Master the carbide device and apply the exact threshold according to the screed binder.
Painted floors and resins: substrate moistureWhen you cannot wait: epoxy barrier, conditions and what it does not solve
Distinguish the real capabilities of a moisture-barrier primer from the illusions of an untenable schedule.
Painted floors and resins: substrate moistureOpening the substrate: shot blasting, diamond grinding and surface laitance
Remove cement laitance by shot blasting to ensure the mechanical bond of the resin.
Painted floors and resins: substrate moistureEpoxy or polyurethane: hardness, flexibility, UV resistance and room use
Select the right chemistry between the mechanical rigidity of epoxy and the UV-resistant flexibility of polyurethane.
Painted floors and resins: substrate moistureMixing correctly: exact ratio, open time, temperature and lost batch
Calculate the pot life and control the mixing to avoid thermal runaway.
Painted floors and resins: substrate moistureJoints: reproduce a screed joint, never cover it, and treat it
Respect the layout of the contraction joints without ever restraining the structural movements of the slab.
Painted floors and resins: substrate moistureThe floor-wall junction: skirting upstand, coved fillet and a room that can be washed down with a jet
Form continuous corner coves to ensure the watertightness of rooms that are washed down with high-pressure jets.
Painted floors and resins: substrate moistureAnti-slip: slip-resistance class, broadcast aggregate and cleanability
Broadcast calibrated quartz to reach the slip-resistance class without sacrificing hygienic cleaning.
Painted floors and resins: substrate moistureWhen you can walk on it again: foot-traffic time, rolling load and full hardening
Set the through-cure times before heavy traffic from forklift trucks.
Painted floors and resins: substrate moistureThe floor is blistering: diagnosing the cause, liability and full renovation
Identify the osmotic origin of a resin blister in order to establish precisely where insurance responsibilities lie.