Key takeaways
- High roughness prevents falls but makes daily maintenance harder for the cleaning teams.
- The required slip-resistance class depends directly on the intended use of the room and on the fluids present.
- The choice of aggregate and its sealing determine the final relief of the floor covering.
- The operator must validate a sample area with their own washing equipment before execution.
Determining the slip-resistance class according to use and cleanability of the room
On a poured-floor construction site, the painter-applicator faces a permanent physical contradiction: the more grip under the sole increases to prevent slips, the more the surface finish retains dust, grease and wash-water residue. A floor that is too smooth exposes users to accidents in the presence of liquids, but a floor that is too rough destroys cleaning equipment, accelerates soiling and triggers immediate complaints from the client at commissioning.
| Use of the room | Indicative class | Operating environment | Cleaning constraint |
|---|---|---|---|
| Offices, dry corridors, dry technical rooms | R9 | Permanently dry, street shoes | Simple damp sweeping, standard disc scrubber-dryer |
| Communal sanitary facilities, changing rooms, laundries | R10 | Occasional moisture, occasional splashes | Daily cleaning, low-speed discs or microfibre |
| Professional kitchens, mechanical workshops | R11 to R12 | Constant presence of water, oils or grease | Scrubber-dryer with hard cylindrical brushes mandatory |
| Covered external access ramps, washing areas | R12 to R13 | Frequent run-off, risk of aquaplaning | High-pressure washer and industrial suction |
The recommendations of the Swiss Accident Prevention Bureau set the slip-resistance requirements to prevent occupational and public risks. The painter must never choose this class alone during the works. The trade-off between personal safety and maintenance cost lies with site management and the building operator. In a communal laundry or a workshop, imposing excessive roughness without adapting the caretaking equipment inevitably leads to blackened soiling of the recesses within a few weeks.
Mastering the broadcast grain size and having the sample area signed off
The anti-slip texture is created by incorporating mineral fillers into the epoxy or polyurethane resin film. Two workshop methods exist: incorporating fine fillers into the body of the topcoat for a soft texture, or mechanical or manual broadcasting of oven-dried quartz sand onto a still-fresh base coat. The painter strictly checks the grain-size distribution of the grains in order to obtain a uniform roughness across the whole room.
- Application of the base coatSpread the tinted resin with a notched squeegee at the prescribed rate to form a wet film of uniform thickness capable of wetting the aggregate.
- Broadcasting of the aggregateThrow the oven-dried quartz upwards in an arc so that it falls vertically and evenly. For a closed texture, broadcast to refusal until all glossy areas have completely disappeared.
- Sweeping and vacuuming of the excessAfter the resin has fully cured, remove the loose filler with a soft broom, then use an industrial vacuum cleaner to clear the recesses.
- Application of the closing seal coatApply one or two coats of finishing resin by roller to coat the sharp edges of the quartz without completely drowning the anti-slip profile created.
For wet rooms requiring an R11 rating, quartz sands graded between 0.3 and 0.8 millimetres are generally used. The thickness of the final seal plays a decisive role: a topcoat applied with too much material excessively rounds the relief and cancels the anti-slip effect, whereas a seal that is too thin leaves porous, sharp grains that trap dirt and tear out under heavy traffic.
Execution of broadcasting to refusal and dosing of the seal
Obtaining a uniform anti-slip surface on a synthetic resin floor relies on broadcasting to refusal into a still-fluid mass. Any partial broadcasting, often attempted to limit the loading or soften the relief, creates uneven surface finishes, patchy gloss and random slipperiness. The applicator spreads the pigmented resin with a notched squeegee or roller, then throws on the fire-dried quartz or corundum fillers. The worker moves about in spiked shoes so as not to mark the film, throwing the filler upwards in a parabola to obtain an even vertical fall onto the binder.
- Application of the receiving filmSpread the body resin with a spreading comb, observing the nominal consumption to form a receiving bed capable of anchoring the base of the grains.
- Broadcasting of the aggregates to refusalThrow the quartz grains until fully saturated, visible by the disappearance of any wet area. This excess guarantees perfect mechanical locking of each particle.
- Dust removal and removal of the loose surface materialAfter full curing, remove the non-adhering fraction by careful sweeping, then use an industrial vacuum cleaner to extract the dust lodged in the relief.
- Application of the closing coatApply the sealing resin with a lacquer roller or squeegee. This wear coat coats the tops of the grains without filling the cavities of the drainage volume.
The final thickness of the closing seal is the most critical lever in the trade-off between roughness and ease of washing. An under-dosed wear coat preserves excellent initial grip but leaves sharp mineral edges and micro-crevices that retain grease, foul the substrate and destroy cleaning textiles by rapidly tearing out their fibres. Conversely, excessive application of finishing resin buries the asperities, fills the cavities that receive liquids and causes the slip-resistance class of the floor to drop under a film of water. The painter therefore calibrates the consumption per square metre according to the supplier's tolerances in order to stabilise the geometry of the relief.
Cleanability in operation and transfer of responsibility
In the field, pressure from the operating teams sometimes leads the operatives to want to reduce the broadcast grain size or overload the seal in response to anticipated complaints about the hardship of washing. Such an initiative on the construction site constitutes a serious professional fault. Unilaterally changing the specified roughness to simplify maintenance may reduce the machines' pass time, but directly exposes users to same-level falls in areas subject to greasy or wet splashes. The slip-resistance class set in the quote derives from an analysis of accident risks and from the federal directives on occupational safety, which are mandatory requirements that always prevail over ease of sweeping.
| Slip-resistance class | Surface profile | Required maintenance equipment | Constraints for the operator |
|---|---|---|---|
| R9 | Smooth or micro-textured surface | Flat broom, short-pile microfibre, scrubber-dryer with soft discs | Quick drying, washing with usual neutral detergents without mechanical constraint. |
| R10 to R11 | Sealed grain size 0.2 to 0.5 mm | Compact scrubber-dryer fitted with cylindrical brushes | Linting textile mops prohibited; suction of residual waste water essential. |
| R12 to R13 | Grain size 0.4 to 1.2 mm with open relief | High-pressure single-disc machine, hot-water cleaner, hard brushes | Gravity drainage via traps and channels required; longer drying time. |
Handover of the work is accompanied by the transmission of the detailed maintenance notice, annexed to the operating file in accordance with the rules of standard SIA 118. This technical documentation specifies the composition of the authorised cleaning agents, the maximum rotation speed of the washing brushes and the ban on traditional textile equipment from class R10 upwards. By formalising these directives in writing to the operator and to site management at acceptance, the painter closes their intervention within a clear contractual framework, preventing any dispute linked to the visual ageing or soiling of the synthetic covering.
Dispute management: excessive slipperiness or a floor impossible to maintain
Disagreement almost always arises after commissioning. Two scenarios are opposed in the field: the operator notes repeated slips during washing with large amounts of water, or the maintenance service complains of tearing up mop heads and jamming the squeegees of the scrubber-dryer on a covering that has become a veritable sandpaper.
When the operator judges the floor too slippery despite compliance with the specification, the painter must never pour on an additional varnish blindly. The first measure is to require a joint inspection record on site. It must be checked whether the maintenance method complies with the technical data sheets: an unsuitable detergent leaves a greasy film that saturates the roughness and nullifies the anti-slip effect. If the intrinsic slip resistance remains insufficient in view of the safety requirements of the Swiss Accident Prevention Bureau, the remedial work requires mechanical sanding of the existing seal, application of a new epoxy or polyurethane resin film and calibrated broadcasting of corundum or fine quartz before re-varnishing.
Conversely, if the floor retains dirt and destroys the cleaning discs, the roughness is excessive in relation to the establishment's maintenance equipment. Two technical solutions remain possible. The first is to apply by roller an additional coat of unfilled film-forming seal to partially bury the heads of the grains, which softens the profile without making it smooth. If the original texture contains aggregates that are too coarse, causing destructive snagging, light sanding with diamond discs to shave off the quartz peaks, followed by degreasing and a closed finish, restores cleanability in accordance with the rules of standard SIA 118.
Frequently asked questions
How should you react if the client refuses to sign the anti-slip sample?
The applicator must give notice of their refusal to carry out the finishing coat as long as the choice has not been fixed in writing. Applying a roughness without formal agreement exposes the company to complete rework at its own expense. Record the absence of a decision in the site diary and send a formal notice recalling the direct conflict between grip and cleanability.
Can a floor be made anti-slip using only glass microbeads?
Glass beads or polymer powders incorporated into the seal provide a light roughness suited to dry rooms or office areas. On the other hand, for workshops, professional kitchens or ramps exposed to water and grease, only broadcasting to refusal of quartz or emery sand guarantees a lasting slip-resistance class under heavy traffic.
Why does the scrubber-dryer leave black marks on a broadcast resin?
A rough resin tears off the soft rubber blades of the squeegees or prematurely wears out unsuitable brushes. Dirt lodges between the quartz grains if the suction pressure is insufficient. The operator must be instructed to use medium-hard nylon-bristle brushes and an emulsifying detergent, rather than abrasive textile discs that fray on the asperities.
How do you correct uneven broadcasting that shows smooth areas?
Gaps in the aggregate create dangerous slippery traps. Local broadcasting onto an already cured resin is prohibited. The defective area must be delimited, mechanically sanded until the varnish is removed, re-primed with fresh resin, then re-broadcast to refusal. After curing and vacuuming of the excess, a new seal coat guarantees visual and mechanical uniformity.
Texts and standards cited
- norme SIA 118General conditions for the execution of construction works and handling of disputes relating to defects in the work