Skip to content
Website
🧱 CFC 272Painted floors and resins: substrate moistureChapter 6 of 10 in the section

Joints: reproduce a screed joint, never cover it, and treat it

On a mineral screed, the contraction joint dissipates the mechanical and thermal stresses of the substrate. In this chapter you will learn why covering this gap with a rigid resin systematically leads to tearing of the floor film, and how to carry out, in accordance with the rules of the trade, the exact reproduction of the opening using a profile or a flexible sealant.

Key takeaways

  • Any contraction joint covered with a rigid film is reproduced as a crack at the surface.
  • The SIA 251 standard prescribes faithfully carrying the joints of the substrate through into the covering.
  • A rigid bridging made of filled resin transfers the stresses and breaks the local bond.
  • Compliant treatment uses a suitable backing rod completed with a continuous elastomeric sealant.

The unavoidable reproduction of the contraction joint through the floor resin

The contraction joint, sawn or formed in the mineral screed, is not a flatness defect that the applicator may conceal. It is an indispensable kinematic discontinuity, designed by the screed layer to absorb the initial shrinkage of the hydraulic binder and to concentrate the deformations caused by hygrometric or thermal dimensional variations. A levelling coat or a film of epoxy or polyurethane resin poured continuously over this line without any special provision directly undergoes the full amplitude of the movement between the two independent slabs.

Floor resin has a high modulus of elasticity and an elongation at break that is often lower than the local stresses generated at the saw cut. When the lips of the joint move apart, even by a fraction of a millimetre, the tensile stress concentrates in the millimetre-thin thickness of the surface coating. Unable to dissipate this mechanical energy over a wider area, the polymer film ruptures through the classic phenomenon of reflective cracking of the substrate joint. This straight, visible and sharp tear runs through the whole thickness of the film down to the substrate.

Reflective cracking of the joint
Spontaneous rupture of a floor covering poured in one piece over a substrate joint, caused by the direct transmission of shear or tensile stresses that the film cannot withstand.

Expansion, settlement and separation joints of the structural work and of the screed must be reproduced correspondingly in the applied floor covering.

norme SIA 251

Compliance with the requirements of the SIA 251 standard obliges the applicator to make the layout of the surface cuts of the synthetic covering coincide with that of the underlying screed. Concealing a contraction joint in order to obtain a visually monolithic surface engages the professional liability of the painter-applicator, because the defect is certain to occur in the short term.

Methodical reproduction of the substrate joints using a profile or flexible sealant

Correct handling of a contraction joint relies on opening it mechanically, cleaning it carefully and carrying it through geometrically, strictly, across all the layers of the paint or self-levelling resin build-up. The applicator must locate and mark the exact position of the saw cut before any sanding, shot-blasting or application of the pore-sealing primer. Two main techniques make it possible to ensure the technical continuity of the work without risking the tearing of the edges.

Comparison of joint treatment methods beneath floor resin
Technical solutionPreferred field of useMechanical advantagesApplication constraints
Prefabricated mechanical profileHeavy traffic, continuous passage of pallet trucks or rigid trolleysAbsolute protection of the resin edges against impact and ravellingPerfectly aligned installation on fresh screed or precise anchoring in a dedicated groove
Flexible elastomeric sealantPedestrian traffic, light traffic, technical and commercial premisesExcellent liquid tightness, application adaptable on renovation construction sitesRequires a calibrated backing rod, sensitive to very severe localised indentation
  1. Locating and opening the saw cutLocate the joint precisely before applying the system. Open the slot with a diamond grinder fitted with extraction at source to obtain vertical, parallel, dust-free sides.
  2. Application of the floor system and clean stopApply a reinforced masking tape or insert a separating strip to stop the body coat on each side without filling the joint gap with the poured resin.
  3. Installing the cellular backing rodForce in a round closed-cell polyethylene foam profile with a diameter 25 per cent greater than the width of the gap, in order to prevent the sealant from bonding on three sides.
  4. Bonding primer and injection of the elastomeric sealantApply a reactive primer to the sides of the slot, then extrude a polyurethane or polymer sealant with a high modulus of elasticity. Strike off the excess with a flexible, slightly concave spatula to protect the bead from surface wear.

Application of the flexible sealing: cellular rod, primer and sealant

Treating a contraction joint within the thickness of the resin film requires a total dissociation between the movement of the screed lips and the finishing covering. According to the SIA 251 standard, the joints present in the substrate must be reproduced congruently in the floor covering. For the painter-applicator, the work begins with opening the lips of the joint with a grinder fitted with a diamond disc, to remove the friable edges resulting from the screed layer's initial sawing and to guarantee perfectly sound, vertical bonding sides, cleaned of dust by industrial extraction.

  1. Calibrating the depth and installing the backing rodForce in a closed-cell polyethylene foam cellular rod with a diameter approximately 25% greater than the width of the groove. This rod prevents the sealant from bonding to the bottom of the groove and limits the elastic working to the two vertical sides. The depth left for the sealant must correspond to the manufacturer's elasticity recommendations.
  2. Application of the specific bonding primerApply with a fine brush a reactive bonding primer, one-component or two-component depending on the sealant selected, to the dust-free lateral faces. Take care not to overflow onto the adjacent areas of the floor where the body resin will be poured, otherwise zones of non-adhesion of the film will be created.
  3. Extrusion and tooling of the elastomeric sealantExtrude the polyurethane or MS polymer sealant continuously, without trapping air bubbles. Press the material firmly against the sides using a spatula dipped in a neutral smoothing agent, creating a slightly concave surface located one to two millimetres below the floor surface to avoid early matting under the wheels of vehicles.

In heavy-traffic premises, in particular those subject to frequent passage of forklift trucks with hard polyamide wheels, the flexible sealant reaches its limits under dynamic indentation. The applicator must then specify the incorporation of a prefabricated metal profile in aluminium or stainless steel. This profile, mechanically anchored into the lips of the screed after forming the gap, incorporates a replaceable elastomer insert and ensures the geometric continuity of the floor while protecting the sharp edges of the poured resin against mechanical delamination.

Dynamic behaviour of the lips and selection of the treatment method

Reflective cracking results directly from the differential kinematics of the adjacent slabs. The elasticity of a conventional epoxy floor resin only very rarely exceeds a low percentage of elongation at break, whereas the residual shrinkage of the screed or the heating cycles impose localised linear deformations far greater than the tensile strength of the polymer. Taking the level of loading into account determines the application technique on the construction site.

Behaviour of the jointing systems according to the demands of the room
Technique appliedRetention of the resinResistance to rolling loadsMajor pathological risk
Filling with epoxy mortar and glass clothTotal failure by linear crackingNone after rupture of the filmFlaking, strip-wise detachment and penetration of liquids
Elastomeric sealant on PE rodIntegrity of the floor resin preservedModerate (pneumatic or soft castors)Tearing out of the sealant under the passage of rigid metal wheels
Added mechanical aluminium profileExcellent, clean delimitation by profileHigh to very high (handling equipment)Flatness defect if the finished level is not perfectly flush

During the preparatory stages, the painter-applicator must visually check the saw-cut lines of the screed before starting the levelling coat or pouring the wearing layer. Any joint prematurely hidden by sanding dust or a primer saturated with quartz must be marked with wall reference marks or surveyed geometrically. This line makes it possible to cut into the freshly polymerised resin again exactly above the underlying saw cut, thus restoring the decompression gap before the final injection of the flexible sealing sealant.

Bridging damage: methodology for repairing a cracked resin

The appearance of a continuous straight tear in a poured floor covering almost always reveals the faulty covering of a contraction joint. Under the effect of residual shrinkage and thermal variations of the screed, mechanical stresses concentrate at the initial cut of the substrate. The synthetic resin, unable to absorb such an amplitude of elongation in direct bond, undergoes reflective cracking of the joint. Faced with this defect, surface filling or simple localised sanding is bound to fail: it is essential to restore the mechanical function of the contraction joint by recreating a genuine open joint.

  1. Diagnosis and marking outLocate the exact alignment of the original contraction line in the screed. Mark two parallel reference lines on either side of the crack to delimit the extent of the future joint profile or sealing chamfer.
  2. Sawing and mechanical clearingOpen the crack with a diamond grinder under industrial extraction until the discontinuity of the underlying screed is found again. Cut out the detached resin on either side of the edge over a minimum width of fifteen millimetres in order to reach a perfectly bonded substrate.
  3. Reconstitution of the lipsCarefully clean the walls of the cut by dust removal with an industrial vacuum cleaner. Reconstitute the damaged edges using a non-shrink epoxy resin mortar to guarantee straight, parallel edges, suitable for receiving the sealing system.
  4. Flexible sealing or profileAfter complete polymerisation of the repair mortar, insert a cellular polyethylene foam backing rod to delimit the depth and prevent bonding on three sides. Apply a bonding primer to the sides, then inject a flexible elastomeric sealant or install a mechanical profile suited to the traffic.

Handling defects in resin requires informing the site management immediately upon the appearance of a suspicious linear crack. In accordance with the principles of the SIA 251 standard governing poured floor coverings and screeds, reproducing the substrate joints up to the finished surface is a strict technical obligation. No warranty on the work covers a crack originating from a joint covered without prior decoupling.

Frequently asked questions

Can a synthetic or glass-fibre mesh be embedded to erase a contraction joint beneath the resin?

No. Embedding a glass tissue or a reinforcing mesh does not compensate for the shear movements and thermal opening of the screed. The reinforcement shifts the stress to its edges or tears quickly under mechanical fatigue, causing reflective cracking of the joint. The SIA 251 standard prescribes faithfully reproducing the substrate joints through the resin in the form of flexible joints or suitable profiles.

What should be done if the screed shows random cracks located outside the contraction joints?

Unlike contraction joints, which must remain mobile and open, passive random shrinkage cracks must be consolidated before the resin is applied. They should be opened by disc-cutting, transverse metal staples should be placed every twenty to thirty centimetres, and they should then be filled to refusal with a fluid epoxy injection resin filled with oven-dried quartz sand.

How can the resin film be neatly connected to an added metal joint profile?

The mechanical profile in aluminium or stainless steel must be fixed mechanically into the screed before the floor system is applied. The perforated flange of the profile is bonded with epoxy resin. The painter applies the body coat until it lies strictly flush with the upper edge, in elastomer or metal, of the profile, protecting the removable central part with a robust adhesive tape.

Must the flexible sealant be applied before or after the resin finishing coat?

The elastomeric sealant must be applied after the resin layers and their protective varnish have fully hardened. If the varnish covered the flexible sealant, it would crack immediately at the surface under the first dynamic loads. The edges of the joint must be masked with clean adhesive tape, dusted off, primed on the vertical edges, then sealed and tooled flush with the covering.

Texts and standards cited

  • norme SIA 251Specifications for screeds and poured synthetic resin floor coverings
  • norme SIA 118General conditions for the execution of construction work and handling of notices of defects

In the same section