Skip to content
Website
🧱 CFC 272Painted floors and resins: substrate moistureChapter 5 of 10 in the section

Mixing correctly: exact ratio, open time, temperature and lost batch

This chapter gives the painter-applicator the exact method for dosing, stirring and splitting two-component floor resins. You will learn to set the stoichiometric ratio on the scale, to eliminate uncured zones by systematic transfer to a second container and to size each batch so as to avoid thermal runaway of the resin in the bucket.

Key takeaways

  • Weighing on an electronic scale guarantees the exact stoichiometric ratio and tolerates no volumetric approximation.
  • Mixing at slow speed followed by a complete transfer to a second container eliminates any uncured component left on the walls.
  • Ambient temperature and the mass effect drastically reduce the open time available for the mix.
  • The size of each batch is calculated strictly according to the application output of the crew deployed.

Electronic weighing and systematic transfer to guarantee curing

On an epoxy or polyurethane resin floor, hardening does not result from the evaporation of a solvent or of water, but from a stoichiometric chemical reaction between the base resin and its hardener. If the molecules are not combined in the exact proportions prescribed by the manufacturer's data sheet, polymerisation remains incomplete. Too little hardener leaves a soft, tacky and chemically vulnerable film, which will be marked by heels and pallet trucks. Conversely, an excess of hardener produces a brittle, glass-like skin, prone to premature micro-cracking and to delamination through loss of adhesion.

  1. Separate weighing on a clean scalePlace a clean, dry plastic bucket on an electronic scale and tare it. Pour in the resin (component A) first up to the required weight, then add precisely the mass of hardener (component B) specified by the manufacturer, tolerating no more than one per cent deviation.
  2. First slow mechanical mixingInsert an electric mixer fitted with a helical paddle designed for resins. Stir at slow speed, between three hundred and four hundred revolutions per minute, for two to three full minutes. Excessive speed traps air bubbles that cannot be removed afterwards.
  3. Transfer to a second containerPour the entire mixed product into a second clean bucket. This essential step prevents pure resin or pure hardener stuck to the walls or the bottom of the first bucket from ending up on the screed as patches that will never cure.
  4. Second homogenising mixResume mechanical stirring in the second container for a further sixty seconds. Make sure the paddle sweeps the bottom without scraping the walls violently, until a perfectly uniform colour with no streaks is obtained.
Mandatory transfer
An operation consisting of emptying a first mixing container into a fresh bucket in order to mix a second time. It removes the risk of incorporating unhomogenised residues left stuck to the walls of the initial bucket.

Controlling open time and anticipating thermal runaway

The reaction between the resin and its hardener is strongly exothermic: it produces heat continuously. As long as the material remains concentrated in the mixing bucket, this heat builds up at the core of the mass, which accelerates the curing kinetics and reduces the time available. This is the mass effect. Within a few extra minutes at summer workshop temperature, a twenty-kilo bucket can rise to more than eighty degrees Celsius, smoke heavily and turn into an unusable glass-like block. To keep the construction site under control, the painter-craftsman must adapt the batch volume to the temperature prevailing at floor level and in the room.

Indicative open time in the bucket and application window according to temperature
Ambient temperatureTime in bucket (mass effect)Spreading time after pouringRecommended batch size
+10 °C45 to 55 minutes60 minutesComplete kit of 15 to 20 kg
+20 °C20 to 30 minutes35 to 45 minutesHalf kit or 10 to 12 kg
+28 °C10 to 12 minutes15 to 20 minutesSmall batches of 5 to 6 kg

To stop this destructive temperature rise, the basic rule on the construction site is to pour the mixed product onto the substrate immediately once mixing is finished, in regular beads. By spreading over the mineral screed in a thin layer of a few tenths of a millimetre up to two millimetres, the resin dissipates its heat into the concrete and regains its nominal maximum open time. A mixed bucket is never left waiting on the floor while answering the phone or preparing a strip of masking.

Sizing batches and pacing the installation

On synthetic floor covering construction sites, the most frequent mistake remains overconfidence in the volume mixed. Preparing a twenty-five-kilo container for a single worker with a roller guarantees a technical failure: after fifteen minutes, the core of the bucket heats up, the viscosity runs away, and the product starts to stiffen while half of the volume is still to be spread. The maximum quantity prepared per pass is never decided from the capacity of the tub, but from the area the painter can apply, deaerate and finish at the edges within a strict ten to fifteen minutes. As soon as the resin is poured as a puddle or drawn with a notched rake onto the screed, its thermal kinetics change radically: the mass spreads into a thin layer, the heat is released directly into the mineral substrate, and the real open time on the floor is preserved. By contrast, the liquid standing at the bottom of the bucket retains its specific heat and polymerises at an exponential rate.

Indicative batch sizing according to crew and temperature
Crew assignedAmbient temperatureSpreading toolMaximum weight per batchTime to empty the bucket
1 painter alone10 °C to 15 °C12 mm polyamide roller5 kg to 8 kgLess than 10 minutes
1 painter alone18 °C to 22 °C12 mm polyamide roller3 kg to 5 kgLess than 7 minutes
2 workers (1 applicator, 1 mixer)18 °C to 22 °CNotched squeegee and spiked roller10 kg to 15 kgLess than 5 minutes
3 workers (continuous chain)25 °C and aboveNotched squeegee and spiked shoes8 kg to 10 kgLess than 3 minutes

The rotation of the buckets demands rigorous logistics between the weighing station and the applicator. The mixer operator cleans the mixer paddle between each batch and begins the next weighing only when the applicator starts deaerating the zone in progress. Systematically using two sets of containers avoids contaminating a fresh mix with residues that are already polymerising and stuck to the walls, which would act as uncontrolled starting points for curing.

Thermal influence of the substrate and treatment of the gelled batch

The air temperature on the construction site almost never matches the mass temperature of the slab. In a basement or in an unheated communal car park, an ambient temperature measured at 18 °C can mask a mineral substrate at 10 °C. This inverse thermal gradient distorts the open time: the resin cools instantly on contact with the slab, its viscosity rises abruptly, hindering the closing of the film and the degassing by the spiked roller. Conversely, on a flat roof or in front of a south-facing glazed bay, a slab heated by solar radiation triggers lightning-fast curing. The craftsman must absolutely measure the surface temperature of the concrete with a contact or infrared thermometer before authorising the first weighing.

Air humidity interacts critically with freshly applied resin. If the slab is at a temperature close to or below the dew point calculated from the construction site's hygrometric station, invisible micro-condensation settles on the binder during its polymerisation. On an epoxy resin, this condensation produces a surface carbamate, often called amine blushing, which leaves a whitish, sticky and hydrophilic film that rules out any finishing coat without prior sanding. On a polyurethane system, water reacts with the isocyanate groups to release carbon dioxide, causing the resin to foam or to blister in the form of micro-bubbles trapped in the film.

Crisis protocols: amorphous resin, runaway and floor repair

A two-component resin that is badly dosed or badly homogenised never polymerises over time. If the film remains tacky or soft after the theoretical curing time, no overcoat will compensate for the defect of the underlying film. The incomplete chemical reaction leaves free monomers that migrate, prevent any subsequent adhesion and destroy mechanical strength. Faced with an uncured batch, the only outcome consistent with the recognised rules of the trade is the complete removal of the contaminated zone.

  1. Immediate removal of a batch in runawayAs soon as a bucket heats abnormally, smokes or gives off an acrid smell, carry the container immediately out of the building into the open air. Place it on an inert surface, away from any combustible material, and never pour water into it, to avoid corrosive splashing.
  2. Scraping and mechanical stripping of the tacky filmRemove the soft mass with a spatula or a metal scraper, limiting its spread. Continue with aggressive mechanical stripping by low-speed diamond grinding, using a coarse-grit abrasive to strip down to sound, unimpregnated concrete.
  3. Degreasing and reopening of the mineral substrateClean the exposed area with a suitable solvent to dissolve the greasy residues of uncured amine, then vacuum with an industrial machine fitted with absolute filtration. Check that the surface regains a uniform porosity before any new impregnation.

In the event of a forced stop caused by a gelled batch on the substrate, delimit the restart along an existing contraction joint or create a clean edge with thick masking tape. Sand down the excess thickness once fully cured before connecting the next batch, to avoid any visible demarcation at the junction.

Frequently asked questions

Can an epoxy resin that has stayed tacky be rescued by heating it?

No. If the mixing ratio is incorrect or the transfer to a second container was omitted, adding heat does not activate any missing chemical reaction. Heat only accelerates the polymerisation of a balanced mix. A resin that is still tacky after forty-eight hours at normal temperature has an irreversible stoichiometric deficit. It must be completely scraped off, mechanically stripped down to the raw mineral substrate, then cleaned with solvent before a new, rigorously weighed pass is applied.

What should you do when a bucket of resin starts to smoke on the construction site?

Thermal runaway comes from an excessive mass confined in a small volume. Grip the container with heat-resistant gloves and take it out of the premises without delay to a ventilated spot clear of any flammable material. Never try to add water or solvent, which would cause violent splashing or toxic vapours. Let the batch cool in the open air before disposing of it as special waste.

How do you clean soiled tools before the end of the open time?

Cleaning of mixer paddles, spatulas and tubs must take place before gelling begins. Use a suitable solvent, such as epoxy thinner or technical alcohol, in a dedicated sealed container. Wipe metal tools carefully with clean, lint-free cloths. Once the resin enters the curing phase, no solvent dissolves the polymer matrix: removal then requires mechanical scraping or destructive thermal burning.

Why is the electronic scale essential compared with the graduated marks on buckets?

The volumes marked on industrial buckets have moulding tolerances that are too imprecise for the chemical tolerances of reactive polymers. Moreover, resins and their hardeners have very different densities, often markedly unequal. Only electronic weighing to the gram guarantees exact compliance with the weight ratio prescribed by the manufacturer's data sheet. A dosing drift of more than two per cent compromises the chemical and mechanical resistance of the system.

Texts and standards cited

  • norme SIA 118General conditions for the execution of construction works

In the same section