Key takeaways
- The single seam allows sheets to slide freely under thermal movement on steep slopes.
- The double seam guarantees mechanical watertightness without restraining the expansion of the metal.
- Tin soldering forms a rigid joint that prevents any linear thermal movement.
- Careful flux cleaning and immediate rinsing determine the lasting strength of the soldered joint.
Choosing and forming the single or double seam according to the thermal clearance
In roof plumbing, metal undergoes large temperature swings between winter frosts and summer sunshine. A zinc-titanium or copper strip several metres long undergoes continuous dimensional change. The seam responds directly to this mechanical constraint by ensuring surface continuity while letting the sheets slide against each other. Unlike a rigid connection, a folded joint creates no concentration of stress that would damage the metal.
- Single seam
- A single 180-degree fold made on the edge of two sheets that interlock with longitudinal sliding clearance, mainly used on steep slopes to channel run-off water.
The single seam is used on roof pitches steeper than 25 degrees, where water runs off by gravity without risk of eddying or standing water. The single fold holds the element mechanically while allowing 3 to 5 millimetres of sliding. In areas exposed to backed-up water or snowmelt, such as recessed gutters or low-pitch edge strips, the double seam becomes mandatory. It has a double fold of the cleats that locks the joint and creates a baffle that is watertight against capillary penetration.
| Type of joint | Minimum pitch | Freedom of expansion | Typical use on Swiss roofs |
|---|---|---|---|
| Single seam | 25° (approx. 47 %) | Full, depending on the direction of the fold | Eaves strips, edge strips, vertical cladding |
| Double seam | 7° (approx. 12 %) | Guided along the axis of the seam | Transverse gutter joints, valley linings |
| Tin soldering | All pitches (excluding expansion) | None (absolute restraint) | Gutter bottoms, outlet spigots, gussets |
Getting tin soldering right and never restraining the metals
The term "soldering" commonly used on construction sites in French-speaking Switzerland in fact refers to soft soldering. The joint is made by capillary action using a tin-lead or tin-copper alloy whose melting point is around 200 to 250 degrees Celsius, well below the melting point of the base metal. Under art. 364 CO, the contractor is liable for the proper execution of the work; this means fully controlling the heating with the plumber's soldering iron so as not to alter the molecular structure of the zinc or copper.
- Flux cleaning and surface preparationBrush the metal edges mechanically to remove the surface oxide layer. Apply with a brush a cleaning flux suited to the metal (zinc-neutralised hydrochloric acid for natural zinc, a specific flux without aggressive acid for pre-weathered zinc or copper).
- Heating and capillary penetrationPlace the tip of the gas-heated copper iron on the overlap, previously tacked. Apply the tin stick against the iron and the sheet. The tip must heat the base metal until the tin melts on direct contact with the sheet and fully penetrates the 10 to 15 millimetre overlap by capillary action.
- Neutralising acid residuesImmediately wipe the still-warm bead with a clean damp cloth to remove flux residues. On zinc, any unrinsed zinc chloride residue causes pitting corrosion that perforates the sheet within a few seasons.
The watertightness check of a soldered joint takes place in two stages on the construction site. First, a careful visual examination: the bead must be smooth and regular, without porosity or gaps, and the tin must show uniformly on the back of the overlap, proving complete fusion across the full width of the joint. Then a physical test by dye penetrant or soapy coloured water is carried out on critical works, in particular downpipe connections, spigots and gutter corners, to certify the total absence of micro-cracks before the roofing elements are laid.
Movement of metal on the roof: why the seam slides and the solder restrains
In pitched-roof plumbing, every metal reacts directly to seasonal and daily temperature swings. In the Swiss climate, the temperature range experienced by an edge strip, a drip edge or a recessed gutter commonly reaches 80 to 100 °C between a morning frost at -15 °C and direct summer sun at +65 °C. Faced with these variations, the plumber never tries to oppose the dimensional changes of thin sheets by force, but channels them by means of decoupled sliding joints.
The incompatibility between soldering and expansion rests on an elementary mechanical principle: soft tin solder rigidly bonds the elements over the entire overlap zone. If a long line of sheet is butt-soldered without an expansion slide, axial tensile and compressive stresses build up within the material. Tin soldering has a shear fatigue strength far below that of the base metal: the joint eventually shears, or the profile buckles, deforming sideways out of its bed and tearing out the perimeter fixings.
| Type of joint | Linear movement allowed | Watertightness | Typical use on a pitched roof |
|---|---|---|---|
| Single seam | Free (depending on seaming clearance and sliding clips) | Protection against dripping (excluding water load) | Eaves strips, drip edges, edge flashings, chimney flashings |
| Double seam | Free along the longitudinal axis with movable clips | Watertight against run-off and capillary rise | Standing-seam roofing, mansard break connections, pitches above 12° |
| Tin soldering (soft soldering) | None (rigid, non-deformable point) | Watertight against standing water and under water-table pressure | Gutter bottoms, outlets, spigots, corner gussets |
The single seam consists of folding a single fold into an opposing groove of the same developed length. It allows the pieces to slide freely into one another while keeping the profiles pressed against the roof boarding. The double seam folds the two interlocked sheets back on themselves into a sealed double fold. This joint offers superior mechanical hold against wind and prevents water passing by capillary rise, while keeping the ability to slide longitudinally if the intermediate fixing clips are installed as sliding clips.
Tin soldering technique, neutralisation and checking of joints
Where the work requires absolute watertightness against running or standing water — such as recessed gutter bottoms, drainage outlets and collector boxes — tin soldering remains indispensable. The metal must be chemically cleaned to dissolve the protective oxide layer and allow the filler metal to wet it. On zinc or copper, a suitable cleaning flux is applied with a brush immediately before heating with the plumber's soldering iron.
- Surface preparation and flux cleaningDegrease and clean the metal mechanically with a non-metallic abrasive pad. Spread a thin, even layer of liquid or gel flux on both faces to be overlapped (minimum overlap of 10 to 15 mm depending on the developed length).
- Tacking and heating with the copper ironTack the joint at points spaced 3 to 5 cm apart to hold the pieces in place. Run the clean, tinned copper tip along the overlap at a constant speed, keeping the ideal working temperature between 250 and 280 °C without overheating the zinc.
- Capillary flow of the tin stickIntroduce the solder stick (generally a 40/60 or 50/50 lead-tin alloy, or lead-free pure tin) directly in contact with the tip and the joint. The molten alloy must penetrate by capillary action across the full width of the overlap and form a full, even fillet at the back of the joint.
- Mandatory neutralisation and immediate cleaningImmediately wipe off flux residues with a damp cloth, then neutralise with plenty of clean water or with a soapy solution. Unrinsed acid residues cause, within a few weeks, perforating crevice corrosion that destroys the base metal.
The watertightness check of the joint takes place in two stages on the construction site. The first check is visual: the plumber checks the uniformity of the tin bead and the absence of porosity, gaps, blowholes or cooling cracks. The solder must show a regular satin sheen without granular tearing.
The second check is operational: for recessed gutters and valleys, a slow, unpressurised water test (temporarily plugging the outlet) makes it possible to monitor the underside of the solder joints for a minimum of 15 minutes. On vertical connections and double seams exposed to the weather, a dye-penetrant check or targeted continuous spraying confirms that no water passes through before the adjacent roofing elements are laid.
Managing joint defects and repair protocols
On a pitched roof, joint defects almost always stem from two design errors: the mechanical restraint of thermal expansion by a rigid solder joint, or the inability of a single seam to hold standing water. When a recessed gutter or a zinc-titanium or copper valley connection tears along a bead, the cause is not a lack of strength of the tin alloy, but the absence of sliding clips or intermediate expansion joints. The metal contracts in winter, puts the solder line in pure tension and causes it to tear through mechanical fatigue. Conversely, a seam crushed with a mallet without leaving longitudinal sliding clearance restrains the sheet in the same way, causing cracking and shearing of the fixing clips.
- Diagnosing the defect and stopping the leaksIdentify whether the crack runs through the solder bead or whether the leak comes from capillary rise in a single seam. In the case of intense greenish or white oxidation, identify a failure to rinse off the cleaning flux.
- Releasing the thermomechanical stressesUnsolder the joint with a heavy iron without overheating the substrate. Cut the metal to create a free space for movement if the line exceeds the permissible lengths without a compensating element.
- Chemical neutralisation and surface preparationRemove residual salts with clean water and a non-metallic abrasive pad. Brush until the sound material is fully exposed, without reducing the thickness of the metal strip.
- Rebuilding the joint according to its movement functionInsert a prefabricated vulcanised expansion sleeve or form a double seam with seamed sliding clips, ensuring the independence of elements subject to temperature gradients.
Faced with these execution defects compromising the durability of the building envelope, the client may exercise the rights provided for in art. 368 CO, requiring the work to be remade at no cost. The plumber must therefore record their watertightness checks and avoid any patching with polyurethane sealant on metal joints.
Frequently asked questions
How do you repair a solder joint cracked by expansion in a gutter?
Never re-solder directly over the existing crack. The repair requires the complete unsoldering of the section, re-cutting the sheets to insert a bellows or an expansion strip of vulcanised elastomer between two metal strips, and then careful soldering of these joints. The upstream and downstream elements must regain their full freedom of movement on their expansion sliding clips.
Why does a single seam let water back up on a low pitch?
The single seam only resists direct run-off water, not water load or capillary suction. On a pitch below the prescribed thresholds, water enters the fold through surface tension or when melting snow accumulates. Only a double seam, fitted if necessary with a non-drying sealing strip, blocks this capillary infiltration.
What are the risks if the flux is not neutralised?
Flux residues, often acidic, remain chemically active in atmospheric humidity. Without immediate rinsing with clean water and thorough wiping after the soldering operation, they attack the zinc-titanium or copper through localised corrosion in the form of deep craters. This perforating attack destroys the plumbing sheet in only a few months, right next to the joint.
Can an existing seamed joint be converted into a soldered joint?
This intervention is strictly prohibited. If the designer or the plumber installed a seam, it was to allow the connected metal parts to expand freely. Soldering this zone removes all functional clearance, restrains the sheet and transfers all the linear expansion onto the fixing clips or onto the material itself, inevitably resulting in a tear through mechanical fatigue.
Texts and standards cited
- CO art. 368client's rights in the event of defects in the work: refusal, price reduction, remedial work, damages; any clause agreed in advance that restricts or excludes the right to have defects remedied is void if the defect concerns a building (para. 2bis, since 1 January 2026).