Key takeaways
- Calculating the developed length requires deducting the bend losses according to the thickness of the metal being formed.
- Planning the bending sequence in advance prevents any mechanical jamming against the apron of the machine.
- The reference sheet and repeatable stops ensure the dimensional consistency of parts produced in series.
- Workshop tolerances determine the precision of the interlocking joints and the straight alignment of profiles installed on the roof.
Calculating the actual developed length and controlling fabrication tolerances
On a pitched roof, a valley flashing, a recessed gutter or a drip edge incorrectly dimensioned in the workshop immediately becomes a costly reject. Unlike joinery adjustments, bent sheet metal can be neither stretched nor planed without impairing the watertightness or the visible appearance of the building. The initial blank must therefore correspond exactly to the unfolded perimeter of the finished part. To calculate this developed length, simply adding up the external dimensions is a systematic error: when crushing or bending at an acute or right angle, the material undergoes elongation on its outer face and compression on its inner face, while the neutral fibre retains its nominal dimension.
- Bend line and bend compensation
- Bend compensation is the arithmetic value deducted from the sum of the external dimensions of a part to absorb the geometric thickening and the stretching of the metal at the formed angle.
The mechanical behaviour varies considerably from one alloy to another. Rolled titanium-zinc of 0.70 mm requires a minimum bending radius to avoid any onset of brittle fracture, especially when the bend is made perpendicular to the rolling direction of the coil. Conversely, half-hard aluminium of 1.00 mm requires a more generous radius, otherwise its powder coating will crack, whereas half-hard red copper of 0.60 mm tolerates very tight folds without loss of structural cohesion.
| Common sheet-metal material | Nominal thickness | Recommended bend radius | Average allowance per 90° bend |
|---|---|---|---|
| Standard titanium-zinc | 0.70 mm | 1.5 to 2.0 mm | 1.2 mm |
| Half-hard copper | 0.60 mm | 1.0 to 1.5 mm | 1.0 mm |
| Coated aluminium | 1.00 mm | 2.0 to 3.0 mm | 1.8 mm |
| Pre-coated galvanised steel | 0.75 mm | 1.5 to 2.0 mm | 1.4 mm |
According to art. 364 CO, the contractor is liable for the proper execution of the works entrusted to them. Workshop fabrication falls directly under this duty of care: a skewed cut or an insufficient fold width compromises the concealed mechanical fixing of the joints and impairs the watertight overlaps essential for the drainage of rainwater.
Establishing the bending sequence and securing repeatability with a template
The ergonomics of a manual or hydraulic press brake impose strict kinematic limits. Each deformation changes the overall bulk of the sheet blank. If the operator does not plan the complete sequence before starting the first pass, the part quickly becomes trapped against the upper beam or strikes the movable apron of the machine. This physical constraint requires bending the internal reliefs and stiffening folds before tackling the closing of the profile bodies.
- Forming the folds and outer hemsFirst make the crushed folds or edge beads on both longitudinal edges of the sheet blank while it is still completely flat.
- Secondary intermediate bendsMake the small water returns, drip edges and stiffening bends, working from the periphery towards the centre line.
- Main structural bendsForm the major angles defining the visible faces, keeping the largest face free of the clamping beam.
- Final closing of the profileFold down the last angle, ensuring there is sufficient clearance to remove the finished part without forcing it on the machine.
For the manufacture of standard series such as sliding cleats, eaves drip edges or ventilation collars, handling the steel rule for each sheet is a major source of cumulative errors. The workshop must work with a reference template cut from an offcut of rigid metal, combined with mechanically adjustable back gauges. The operator validates the first part on this control template before starting the shearing and forming of the entire batch.
Rigorous management of the blanks also limits waste of valuable metal. The ordinance on the prevention of accidents and occupational diseases reminds us that the employer takes the protective provisions and measures that comply with the recognised rules of technology. Systematic deburring of the cut edges, wearing handling gloves suited to sharp edges and correct clamping of the movable stops ensure both the physical safety of the sheet-metal worker and the geometric precision essential for installation on the roof.
Making templates and locking the stops for series production
On a long pitched roof, profitability and watertightness depend on the perfect repeatability of the profiles: eaves drip edges, verge flashings, valleys or fixing strips. When a series of thirty or fifty three-metre sheets has to be formed on a manual or semi-automatic workshop press brake, a setting error of a single millimetre on a stop results in a catastrophic cumulative offset along the slope. The parts no longer interlock, the specified overlap is no longer guaranteed and the concealed fixings no longer fall opposite the roof boards or the eaves fillets.
To eliminate individual marking with a scriber, a source of crack initiation on zinc or powder-coated aluminium, the sheet-metal worker systematically makes a sacrificial template from an offcut of rigid metal or a reference sample twenty centimetres long. This test coupon makes it possible to validate the calculation of the theoretical developed length against the actual behaviour of the machine. The parameters of the clamping beam, the radius of the bending nose and the pressure of the clamp directly affect the bend deduction. If the seaming strip planned at 25 mm comes out at 23 mm after the fold is tightened, the setting is corrected immediately before cutting the valuable material.
| Formed element | Permissible workshop tolerance | Direct consequence on the roof | Workshop locking method |
|---|---|---|---|
| Eaves strip with drip edge | ± 1.0 mm on the developed length, ± 1° on the bend | Gaping of the drip edge against the bargeboard, water infiltration by capillarity | Fixed mechanical back gauge and checking with an angle protractor on a coupon |
| Recessed valley with double fold | ± 1.5 mm on the throat width | Uneven seating of the folds, pinching of the flashing foot, leaves being trapped | Reference template in plywood or 1.5 mm steel sheet to check the hollow profile |
| Verge flashing with water guard | ± 1.0 mm on the upstand height | Visible misalignment along the verge rafter and risk of wind-driven rain overflow | Micrometric stop fingers and symmetrical clamping of the clamping beam |
| Chased-in sealing strip | ± 0.5 mm on the water-shedding fold | Impossible to insert the profile into the masonry chase, or impossible to seal with mastic | Bending a test piece and inserting it directly into a calibrated gauge |
Sequencing the bending kinematics and dimensional checking
The bending sequence determines the technical feasibility of the part. A poorly planned sequence traps the sheet against the apron or strikes the upper apron, forcing the operator to bend the element by hand to free it, which destroys the flatness of the profile. The fundamental workshop principle requires forming the bends from the outside to the inside, keeping the crushed folds or double folds for the end of the sequence, unless these elements have to pass flat under the press blades.
- 1. Rolling or forming the outer hemMake the stiffening hem or bead on the press brake or roll former before any other deformation. The flat profile retains all its rigidity to come up against the back gauge without flexing.
- 2. Bending the seaming folds and secondary upstandsForm the folds at 30° or 45° on the free ends. Depending on the depth of the apron, crush the fold if necessary with the clamp, taking care not to close completely the groove receiving the fixing tabs.
- 3. Making the central bends and changing facesFold down the main angles of the part by turning the sheet downwards or flipping it over to clear the nose of the press brake. Constantly check the clearance of the free profile in relation to the cylinders or the uprights of the machine.
- 4. Final calibration and squareness checkPass the finished profile through a female gauge or check the opening dimensions with a calliper. Three-metre lengths must show a bow of less than 2 mm to guarantee straight alignment on the wall plate.
Handling forming deviations and reworking defective series
A badly developed part is never corrected on the roof. Trying to straighten a crushed fold or to close an angle with a hammer on the verge ruins the flatness of the metal, stretches the material at the bend and destroys the protective layer of the titanium-zinc, copper or powder-coated aluminium. As soon as a dimensional deviation exceeds the permitted forming tolerance of plus or minus one millimetre, the profile must be scrapped in the workshop or set aside on the construction site before any attempt at fixing.
- Immediate stop of cuttingAs soon as a test profile does not fit the control template, stop the cutting machine and the manual or numerical press brake to avoid wasting the coil.
- Checking the bending deductionsCheck on a test offcut whether the actual material allowance corresponds to the radius of the clamping beam used, particularly when changing alloy batch.
- Recalibrating the apron stopsRealign the back-gauge fingers with the steel rule and lock the clamping brackets to prevent any mechanical drift under the bending force.
- Validation on a rigid templateForm a complete sacrificial part and compare it with the workshop template in heavy-gauge sheet or plywood before authorising the resumption of series production.
According to art. 364 CO, the contractor is liable for the proper and faithful execution of the work entrusted to them. Under the rules of the trade of Swiss sheet-metal work, the bending tolerance that can be absorbed by the overlaps and the sliding cleats remains minimal. When the bending sequence proves impossible without collision against the upper clamping beam, the geometry of the profile must be redesigned in the technical office by providing for a splice plate or an intermediate fold, without waiting for the foreman to find himself blocked on the slope with unusable lengths.
Frequently asked questions
How should you react if the bending sequence traps the part against the cheek of the press brake?
Free the sheet without forcing it on the machine, to avoid twisting the clamping beam. Analyse the developed length: the outer fold or the drip edge must generally be made first, then the inner bends, working from the centre outwards. If the geometry blocks access, modify the bending kinematics or split the joint into two parts assembled by seaming or by sliding cleat on the slope.
What maximum dimensional tolerance should be applied when bending a chimney flashing?
For penetration flashings and watertight aprons, the workshop tolerance must not exceed plus or minus one millimetre on the upstand heights and the bending angles. A deviation of two degrees on an inclined face prevents the metal from sitting flat against the masonry, compromising the chase and creating pockets where powder snow accumulates under the profile.
Why is a workshop template mandatory for a series of verge flashings?
The rigid template makes it possible to check the squareness, the dimension of the drip return and the opening of the water fold from the first part off the bench. Since the mechanical stops are subject to repeated vibrations during successive clampings, systematic visual comparison with the control template avoids manufacturing fifty linear metres of profiles that would prove impossible to interlock or align on the bargeboard.
How do you correct a bend angle that opens to 95 degrees instead of the intended 90 degrees?
Do not try to close the profile with a wooden mallet on the construction site. In the workshop, immediately adjust the angular travel of the pivoting apron on the press brake to compensate for the specific springback of the sheet, particularly pronounced on half-hard aluminium. Mark the defective part with a workshop marker and pass it again under the clamping beam with a suitable angle shim.
Texts and standards cited
- CO art. 364obligations of the contractor: liability subject to the same rules as that of the employee; they carry out the work in person or under their personal direction; unless custom or agreement provides otherwise, they procure at their own expense the means, equipment and tools required.