Key takeaways
- Air and zinc vents must be defined in the technical office before fabrication.
- A closed hollow section with no outlet bursts instantly under the thermal expansion in the bath.
- Keeping weld beads symmetrical prevents warping during immersion.
- Touch-ups after on-site welding require abrasive cleaning followed by a high-zinc-content coating.
Venting and drain holes: designing the zinc passage from the workshop drawings onwards
Immersing a metalwork element in a liquid zinc bath at approximately 450 °C tolerates no closed cavity. The air trapped in a hollow section heats up instantly. Its thermal expansion, combined with the instant vaporisation of moisture or acid pickling residues, multiplies the internal pressure to such an extent that the steel tears apart violently. This blast throws masses of molten metal out of the tank, directly endangering the galvanising plant's personnel and destroying the workpiece.
The holes must be integrated into the fabrication drawing on the detail drawings of the steel fabricator or metalworker. Drilling holes with a portable drill on the delivery lorry systematically leads to diameters that are too small or badly oriented. For a railing or a light stair stringer, the hydraulic principle requires two types of openings per closed compartment: inlet and drain holes at the bottom to admit and then drain the heavy zinc, and vent holes at the top to release the air without creating a gas pocket.
| Section or inner diameter of the profile | Minimum diameter of a single hole per end | Corner cut or notch solution |
|---|---|---|
| Up to 40 mm (thin posts, rails) | Diameter 10 mm | Corner bevel at 45° over 12 mm |
| From 40 to 80 mm (handrails, posts) | Diameter 12 to 16 mm | Through-notch opening 25 % of the area |
| Over 80 mm (stringers, light columns) | Diameter 20 mm or two holes of 14 mm | Free diagonal opening at both ends |
To ensure flow without excessive build-up of zinc thickness, the holes must be placed diagonally opposite at the ends of the tubes, flush with the welded plates or caps. If an anchor plate closes the end of a barrier post, the drain hole must not leave an internal step forming a pool: the opening goes through the plate or cuts directly into the tubular wall via a notch machined before welding.
Thermal behaviour in the bath, exposure classes and weld touch-ups
Passing through a bath heated to 450 °C subjects the steel to a thermal shock that instantly releases the internal stresses accumulated during cold rolling and welding. On asymmetrical assemblies, such as a railing made of a heavy flat and thin bars, the uneven expansion causes irreversible warping of the frame. Workshop design must balance the thermal masses and favour discontinuous or alternating weld beads to limit the residual heat input.
The thickness of the protective layer depends directly on the chemical composition of the steel, in particular its silicon and phosphorus content. For metalwork exposed to outdoor alpine weather or to de-icing salt fog, the steel selected must guarantee a regular reaction to form an iron-zinc alloy of at least 70 to 85 micrometres on standard finishing-work parts. A poorly specified steel can lead to over-reactivity, producing a dull greyish coating that is thick but extremely brittle under the impact of assembly tools.
- Cleaning and removal of mill scaleOn the construction site, after fitting welds or adaptation cuts, clean the ground area with a wire brush or a clean abrasive disc to bare-metal standard, with no trace of oxidation or soot.
- Immediate dust removal and degreasingClean the area with a dry solvent leaving no greasy residue to ensure intimate adhesion of the filler product around the remaining thermal zinc.
- Application of the high-zinc-content compoundApply a hot-applied zinc paste or a zinc-dust-rich paint containing at least 90 % dry metallic zinc, overlapping the intact galvanising by at least 15 mm.
- Dry film thickness checkCheck with a magnetic gauge that the thickness of the touch-up film exceeds that of the original layer by approximately 30 micrometres to compensate for its lower density.
Positioning and sizing of vents for hollow bodies
Immersing a closed hollow section in molten zinc instantly brings the trapped air and traces of moisture to the temperature of the liquid. The trapped water immediately turns into steam with a sudden volume expansion, multiplying the internal pressure more than a thousand-fold. Without a through opening, the steel tears violently or the section bursts in the tank. This explosion throws liquid metal several metres, seriously endangering the personnel at the dipping site and irreparably damaging the railing or the workpiece being treated.
Holes are not a minor detail left to the initiative of the galvanising workshop: they must appear explicitly on the metalwork execution drawings. A tubular assembly necessarily requires two distinct openings per sealed compartment: a low opening for the inlet and drainage of the liquid zinc, and a high opening for the escape of air. If one of these passages is missing, an air pocket remains, leaving the inner face without any anti-corrosion protection while creating a buoyancy force that makes the part float and complicates its immersion.
| Closed profile section (mm) | Minimum single vent diameter (mm) | Alternative with two opposite openings (mm) | Required geometric position |
|---|---|---|---|
| Round or square tube up to 40 | Ø 10 | 2 x Ø 8 | At the axial ends or on a concealed edge |
| Square or rectangular tube from 40 to 80 | Ø 12 | 2 x Ø 10 | At the opposite extreme diagonals of the profile |
| Tube or post over 80 | Ø 16 | 2 x Ø 12 | Flush with the plates and mitre cuts |
| Closed frame under infill sheet | Ø 14 | Internal bevel cuts | On each crossbar and post at each node |
Thermal distortion and anti-corrosion repair of assembly welds
Passing through a heated bath causes a sudden release of the residual stresses introduced during cutting, shearing and arc welding. Asymmetrical structures, such as railing rails with bars welded on one side only or light gate frames made of thin sheets edged with thick tubes, are particularly prone to warping. To limit these geometric distortions, the metalworker must balance the weld beads, favour discontinuous welds that remain galvanising-tight, and systematically pre-straighten the elements before they leave for dipping.
The zinc thickness deposited varies with the chemical composition of the steel, in particular its silicon and phosphorus content, and with the thickness of the base metal. For metalwork elements exposed to outdoor weather, in peri-urban or mountain environments subject to de-icing salts, an average protective layer of between 55 and 85 micrometres is usual on standard sections 3 to 6 millimetres thick. Reactive steels known as silicon-killed steels develop thicker but more brittle layers, requiring extra precautions during transport to avoid flaking.
- Mechanical preparation of the modified area on siteAfter a connection weld or an adjustment cut on the construction site, completely remove the slag, spatter and mill scale residues using an angle grinder fitted with a clean abrasive disc, then brush until bright bare metal is obtained with no trace of oxidation.
- Dust removal and degreasing of the substrateClean the ground area and the adjacent zinc edges with a non-greasy volatile solvent to ensure adhesion of the repair system, overlapping the sound coating by a width of at least twenty millimetres.
- Application of the touch-up protectionApply a zinc-rich product containing at least 90 % metallic zinc dust in the dry film, or carry out recharging with zinc wire by hot metal spraying. The dry film thickness of the touch-up must exceed that of the surrounding original galvanising layer by at least 30 micrometres.
Handling disputes, distorted parts and rectification of non-conformities
When the galvanising plant rejects a welded assembly, the cause almost always lies in the absence of visible vents or a clear undersizing of the flow passages. If the metalwork workshop tries to drill hastily on the loading dock without recalculating the flow sections, it risks residual air pockets, destructive explosions on thermal immersion at over four hundred and fifty degrees, or zinc build-ups solidifying inside the tubes. In this situation, the workshop foreman must bring the part back, open the passages to the prescribed diameters and scrupulously clean out internal swarf to avoid any contamination of the bath.
Irreversible thermal distortion is the second most frequent damage on thin infill sheets or asymmetrical rails welded continuously. When differential shrinkage twists a railing post or warps a panel beyond the assembly tolerances, mechanical straightening under a press or with a jack must be done cold with soft aluminium jaws so as not to crack the iron-zinc alloy layer. Any shrinkage heating with a torch is prohibited: it would locally destroy the cathodic protection and vaporise the zinc into toxic fumes.
- Tapped holes and threads clogged with zinc: mandatory rework with a tap or mechanical die without abrasive grinding, followed by immediate application of zinc anti-corrosion paste.
- Drips, tears and build-ups hindering assembly: careful levelling with a smooth file or flat chisel, keeping the intermetallic film without cutting into the base steel.
- Adjustment welds made on the construction site: clean grinding of the bead, wire brushing to bare metal and application in two crossed coats of a zinc-rich paint with suitable dry extract.
Frequently asked questions
How should you react if the galvaniser refuses to dip a railing with no visible vent holes?
Never force the dipping or drill hastily without a drawing. Bring the element back to the workshop to make the inlet and outlet holes at opposite corners according to the hanging direction. Deburr the holes carefully to avoid any dross plug when the molten zinc drains.
What method should be used to straighten a rail bent by the thermal shock of the bath?
Straightening is carried out cold, on a surface plate or with a hydraulic press, inserting dense wooden or aluminium shims so as not to flake the protective layer. Any heat input with a torch is ruled out because it would burn the zinc and destroy the metallurgical bond with the steel.
How should a weld bead made on the construction site to connect a handrail be treated?
First remove the slag and spatter. Then clean the area with a wire brush to the required cleanliness grade, over a width extending twenty millimetres around the bead. Then apply a zinc-dust-rich paint guaranteeing the protective thickness required for the exposure class.
What should you do when the tapped holes of a plate are clogged with zinc on return from dipping?
Run a machine tap lubricated dry or with a neutral grease through again to remove the alloy without damaging the thread profile. Never use a torch to burn off the deposit. Immediately protect the exposed thread with an anti-corrosion compound compatible with the future fixing screws.
Texts and standards cited
- norme SIA 118General conditions for the execution of construction work and handling of defects in the works