Key takeaways
- Every hole drilled on the construction site leaves the steel bare and must be treated without delay.
- Careful deburring and solvent degreasing determine the mechanical adhesion of the touch-up product.
- Use only a paste or paint with a high metallic zinc content that complies with the specifications.
- Touch-up is reserved for small, isolated defects, otherwise the work risks being rejected at acceptance.
Mechanical preparation of the hole and application of zinc on the same day
When installing a barrier, a handrail or a light frame, on-site fitting sometimes requires drilling a bolt hole or cutting back a fixing lug. Hot-dip galvanising forms a protective iron-zinc alloy that works by barrier effect and by sacrificial protection. However, dry drilling or drilling with cutting oil destroys this protection locally: the base steel is left exposed to open air. In French-speaking Switzerland, ambient humidity, morning fog or a simple evening shower trigger surface rust within a few hours, visually polluting the visible faces and starting underlying detachment of the neighbouring zinc.
- Deburring the inside and outside of the holeRemove the metal chips immediately. Run a conical deburring cutter over both faces of the hole to remove sharp edges. A sharp edge prevents the liquid product from properly covering the ridge because of surface tension.
- Complete degreasing of the metalClean the drilled area with a volatile solvent that leaves no greasy residue. Residues of machining oil or cutting paste form a screen that ruins the adhesion of the anti-corrosion binder.
- Applying the zinc-rich compoundApply the touch-up product, concentrating on the inside of the drilled cylinder and on the chamfer, using a fine brush or a swab, overlapping slightly onto the sound, unaffected zinc.
The work must be carried out on the same day as the drilling, before the end of the working shift. Leaving a hole open overnight exposes the bare metal to nocturnal condensation. As soon as a film of brown rust appears, the metalworker must grind or strip the hole again down to bright metal, which needlessly enlarges the mechanical clearance of the fixing and weakens the original coating.
Product compatibility, drying and technical limits of the touch-up
The choice of repair product depends on the climatic conditions and the requirements of the structure. The technical rules for hot-dip galvanising require a product containing a minimum mass fraction of zinc dust of 80 % in the dry extract for touch-up paints. The final dry film thickness of the repair must generally exceed the nominal thickness of the original galvanising by at least 30 micrometres, to compensate for the lower density of the manually applied deposit compared with the molten zinc bath.
| System used | On-site application | Rain-free time (20 °C) | Recommended use |
|---|---|---|---|
| Zinc-rich epoxy paint (2K) | Mix of resin and hardener, applied by brush | 3 to 4 hours | Sawn edges, structural holes, highly exposed parts |
| Single-component zinc-rich aerosol | Prolonged shaking mandatory, two to three crossed passes | 30 to 45 minutes | Light through-holes, blind holes for self-tapping screws |
| Hot-melt zinc stick or paste | Localised heating of the substrate with a soft torch (approx. 300 °C) | Immediate after cooling | Repairs of notched areas, visible flat surfaces, heavy touch-ups |
The time before first exposure to water determines the durability of the treatment. A shower falling on fresh zinc-rich paint displaces the binder and washes out the metallic filler before polymerisation. The substrate must be at least 3 °C above the dew point at the time of application. If installation takes place in cold or misty weather, using a hot-air gun to moderately preheat the part and speed up setting of the binder is a recommended practice on construction sites in French-speaking Switzerland.
Drying, polymerisation and resistance before the first rain
Every adaptation machining operation carried out on the construction site – drilling a guardrail post, adjusting a slotted hole to compensate for a structural work tolerance or cutting a plate – breaks the protective barrier formed during immersion in the liquid zinc bath. The base steel is left exposed to ambient air and condensation water. As soon as the drill passes through the section, the bare edge and hole suffers tearing: micro-burrs of mild steel start immediate oxidation in the form of reddish rust. On construction sites in French-speaking Switzerland exposed to fog and humidity, this phenomenon begins within a few hours.
The time before first exposure determines the durability of the repair. Applying a product a few minutes before a shower causes the binder to wash out or the film to blister. Moisture trapped under an uncured coat generates underlying corrosion that makes the touch-up flake off after a few weeks. The metalworker must plan the treatment according to the weather: the compatible touch-up product must be applied to a substrate whose temperature is at least 3 degrees above the dew point, and then dry free of rain.
- Deburring and chamferingRun a conical cutter to remove burrs and sharp edges that prevent uniform adhesion of the product.
- Degreasing and dust removalBlow out the chips, then clean the inside of the hole with a volatile solvent that leaves no greasy residue.
- Application of zinc-rich productApply the product with a fine brush in the bore and on the lips of the hole, overlapping slightly onto the sound zinc.
- Curing before tighteningAllow it to dry through before inserting the fasteners, to avoid shearing of the film under tightening force.
Limits of on-site touch-up and acceptance thresholds
Liquid touch-up remains a stopgap for installation, with a strictly limited technical scope. The limit of an on-site touch-up stems from the very nature of the process applied cold. Hot-dip galvanising forms zinc-iron alloy layers inseparable from the steel through a continuous metallurgical bond. By contrast, a zinc-rich paint applied cold offers only mechanical adhesion on the brushed metal. When the machining goes beyond simple isolated adjustments, the overall corrosion protection of the light metalwork can no longer match that of the original treatment.
In building metalwork, the total area touched up on a finished part must never exceed half a percent of its surface, with continuous zones of less than ten square centimetres. Heavy cuts with an angle grinder, tubular notching to correct a setting-out error or the multiplication of slotted holes require the part to be sent back to the workshop for stripping and hot-dip regalvanising. When installing guardrails or handrails, the use of wide A2 or A4 stainless steel washers, sometimes backed with a synthetic EPDM washer, makes it possible to tighten to the specified torque without crushing or tearing the protective film on the lips of the hole.
| On-site machining | Corrective action required | Admissibility on the construction site | Corrosion risk |
|---|---|---|---|
| Single fixing hole (diameter 8 to 14 mm) | Deburring, degreasing, zinc-rich product by brush | Admissible on the same day in dry weather | Low if the minimum dry thickness is reached |
| Slotted hole adjusted with a grinder | Careful chamfering, two coats of zinc-rich product | Admissible with complete drying before tightening | Medium if the washer tears the fresh film |
| Trimming of a plate or cutting of a rail | Light grinding, brushing, three crossed coats | Tolerated on clean cuts not visible from outside | High on sharp edges exposed to rain |
| Heavy notching or adaptation welding | Mechanical cleaning, stripping and regalvanising | Formal rejection on site: mandatory return to the workshop | Critical, with rapid detachment and rust runs |
Acceptance of the work under the SIA 118 standard penalises any premature trace of oxidation with an immediate notice of defects. The appearance of rust halos around the fixings a few weeks after installation directly engages the metalworker's liability. By systematically recording every touch-up in the daily reports and rejecting decorative aerosol cans, the team preserves the value of the construction and ensures the conformity of the work in the face of checks by the site management.
Claims management: rust runs and rework of faulty holes
A neglected touch-up on a hole or a plate bevel shows itself without delay: with the first bad weather, water seeps into the hole, oxidises the bare steel and causes a ferruginous run along the guardrail posts as far as the slab edges, natural stone thresholds or façade renders. When damage occurs, the metalworker must intervene immediately to stop the spread of corrosion and avoid claims for damages from the site management for deterioration of adjacent works.
- Immediate cleaning of soiled substratesWash off rust marks on concrete, tiling or sheet-metal work without delay using a suitable solution, often oxalic-acid based, then rinse abundantly with clean water before the iron oxide becomes permanently embedded in the pores of the substrate.
- Removal of fixings and mechanical remediationDismantle the bolting or loosen the anchor to free the hole completely. Remove incipient rust inside the bore and on the sharp edges using a wire swab mounted on a screwdriver and a non-woven abrasive disc, until bright bare metal is regained.
- Degreasing and reapplication of a zinc-rich compoundRemove dust, then degrease carefully with clean volatile solvent. Apply a zinc-dust-rich paint with a high dry extract, filling the full depth of the hole with a round brush, rather than settling for a superficial aerosol film.
- Shelter and complete dryingProtect the reworked area with a temporary watertight cap if rain threatens before the end of the rain-free drying time, to prevent any further washing out of the binder.
Frequently asked questions
Is a shiny zinc spray can from a shop enough to touch up a hole on site?
No. Decorative finishing aerosols in aluminium or light zinc contain too high a proportion of resin and too low a metallic zinc content to provide genuine sacrificial protection. On the construction site, the metalworker must use a zinc-rich product with a high dry extract, certified for anti-corrosion touch-up, applied by brush to deposit the minimum required dry film over the whole steel edge.
How long must you wait before tightening a bolt on a touched-up hole?
You must wait for the protective film to cure completely, generally between four and twelve hours depending on ambient temperature and humidity. Premature torque tightening crushes the still-fresh resin, expels the zinc from the contact zone under the washer and leaves the steel bare again through shearing, starting under-head corrosion at the first outdoor condensation.
What should be done if a hole on the construction site was exposed to rain before the zinc dried?
Water degrades the emulsion of the binder and causes immediate washing out of the touch-up, leaving the steel edge without active defence. The fixing must be removed, the soaked layer eliminated with a wire brush or swab, the part dried with hot air, the area degreased and the zinc-rich compound reapplied in full, protecting the assembly from any new shower.
Can a wrongly positioned guardrail hole be concealed with just filler and a zinc touch-up?
No, this practice is strictly non-compliant for an outdoor structure. Filler provides no sacrificial galvanic protection and moisture eventually stagnates in the cavity, causing invisible internal crevice corrosion. Any erroneous hole must be filled mechanically by clean ground-flush welding in the workshop before anti-corrosion retreatment, or receive a watertight bolted reinforcement piece treated according to the rules of the trade.
Texts and standards cited
- norme SIA 118General conditions for the execution of construction work and management of defects in the work
- code des obligationsGeneral rules on the contract for work and on the contractor's liability for defects in the work