Skip to content
Website
🧱 CFC 281Cement or anhydrite screed: selection and executionChapter 1 of 10 in the section

Cement or anhydrite: room humidity, drying, shrinkage and planned floor covering

The choice between a cement binder and a calcium sulphate binder determines the durability of the floor assembly and compliance with the construction site schedule. This chapter enables you to select the appropriate binder according to the water exposure class of each room, precisely plan shrinkage joints, and schedule the release moisture measurement.

Key takeaways

  • Calcium sulphate loses its mechanical strength when exposed to continuous moisture.
  • Cement screed remains mandatory for communal laundry rooms, technical rooms and outdoor areas.
  • Anhydrite allows surfaces without dividing joints up to three hundred square metres.
  • Carbide bomb moisture testing remains the sole official validation prior to installation.

Deciding on the binder choice according to the moisture exposure of the rooms

Standard SIA 251 governs the design and execution of screeds inside buildings. The first selection criterion is based on the physical-chemical behaviour of the binder in the presence of water. A calcium sulphate-based screed, commonly called anhydrite screed, reacts reversibly with moisture: if it absorbs residual water or a prolonged accidental inflow, its crystalline matrix softens, leading to a drastic drop in its compressive and flexural strength. Conversely, cement screed retains all of its mechanical cohesion and surface hardness under continuous immersion.

Binder decision matrix by room use according to standard SIA 251
Room useWater exposureRecommended binderSpecial execution requirements
Living room, bedrooms, hallwaysNone to occasionalCalcium sulphate or cementAdvantage for anhydrite for perfect embedding of heating pipes and flatness.
Closed kitchen, guest WCLow and occasionalCalcium sulphate or cementSurface protection required under the setting adhesive in case of anhydrite.
Bathroom without floor drainModerate (splashes)Calcium sulphate or cementWaterproofing system under tiling is mandatory for anhydrite.
Walk-in shower or private laundry roomHigh with floor drainCement exclusivelyAnhydrite prohibited by standard SIA 251 in areas with direct drainage.
Underground garage, technical room, outdoorPermanent or severe humidityCement exclusivelyRisk of infiltrations incompatible with calcium binders.

Controlling shrinkage, joint layout and drying kinetics

Traditional cement screed undergoes marked hydraulic shrinkage during the evaporation of its excess mixing water. This dimensional phenomenon creates internal tensile stresses that cause cracking and characteristic curling at the corners of the slabs. To neutralise these tensions, standard SIA 251 mandates systematic cutting into regular panels. Shrinkage joints must be sawn or profiled every twenty to forty square metres, with rigorous attention to door thresholds and internal corners.

Conversely, calcium sulphate flowable screeds exhibit almost zero shrinkage during the formation of their gypsum crystals. This remarkable dimensional stability allows the pouring of continuous, single-pour surfaces reaching up to three hundred square metres without any intermediate dividing joints, provided simple geometries are maintained and peripheral edge insulation strips are respected. The screed layer thus eliminates the risk of joint reflection under thin floor coverings.

Regarding drying, anhydrite screed allows the heating-up protocol to be initiated earlier than cement mortar, accelerating vapour evacuation. However, its fine porosity makes final-cycle diffusion slow in saturated environments. The acceptance criterion for installation depends strictly on the destructive calcium carbide bomb measurement (CM method). On underfloor heating, calcium sulphate requires a residual moisture content of less than or equal to 0.3% CM for parquet and 0.5% CM for tiling, compared to 1.5% CM on a cement screed with tiling. Starting any floor covering installation without a written CM measurement protocol relieves the flooring installer of liability and engages the responsibility of the screed layer.

Room-by-room decision matrix according to standard SIA 251

The choice between a calcium sulphate (anhydrite) screed and a cement screed does not depend solely on the speed of execution or the cost per square metre. According to standard SIA 251, the destination of each room and its level of exposure to ambient moisture or water splashes determine the admissible binder. Anhydrite presents a critical structural sensitivity: upon prolonged contact with stagnant water or in the event of continuous infiltration, the gypsum partially dissolves, loses its crystallisation and suffers a drastic drop in its compressive and flexural tensile strength.

Suitability of binders according to water stress in rooms (standard SIA 251)
Room useWater exposureCement screedAnhydrite screed (calcium sulphate)
Bedrooms, living rooms, officesNone to occasional (cleaning)Compliant (fractionation from 40 m²)Optimal (large areas without joints, flowability)
Private residential kitchensModerate (occasional splashes)CompliantPermitted with waterproofing under watertight tiling
Bathrooms with bathtub/standard showerFrequent but temporaryRecommendedPermitted under strict condition of a liquid waterproofing system
Walk-in showers (floor-level)Direct and repeatedPrescribed (essential under drain)Prohibited or strongly discouraged in sloped areas
Communal laundry rooms, technical water roomsHigh to permanentPrescribedFormally excluded (risk of stagnation)
Garages, basements on grade without waterproofingRising damp or runoffPrescribedExcluded (degradation by underlying moisture)

On intermediate slabs in dry areas, the calcium sulphate self-levelling flowable screed outperforms cement due to its almost total absence of dimensional shrinkage. It allows continuous pours up to several hundred square metres without intermediate dividing joints, apart from door openings and strict compliance with building expansion joints. Conversely, as soon as a floor drain exists without a prefabricated shower tray, cement screed is required to shape the slopes and resist any potential failure of the waterproofing beneath the tiling.

Drying kinetics, heating-up and installation authorisation

The kinetics of hardening and residual water evacuation diverge fundamentally between the two materials. Calcium sulphate screed develops no significant hydraulic shrinkage during its setting: it does not curl and exerts no parasitic tension on peripheral insulation. Furthermore, its perfect thermal conductivity and complete embedding of underfloor heating pipes allow early thermal commissioning. According to the manufacturer's guidelines and standard SIA 251, functional heating-up of an anhydrite flowable screed can start as early as the seventh day following pouring, compared to at least twenty-one days for a traditional cement screed.

  1. Surface sandingMandatory mechanical removal of the surface film (laitance) on the anhydrite screed as soon as the substrate is walkable, generally between 48 hours and 7 days after installation, in order to open the porosity and accelerate the evaporation of mixing water.
  2. Heating-up cycleRigorous execution of the thermal protocol on the manifold: supply at 25 °C for three days, then increase in daily increments of 5 °C up to the maximum target temperature, maintaining it for at least four days, followed by controlled cool-down.
  3. Release moisture measurementMandatory execution of the destructive calcium carbide bomb measurement (CM method) on a sample taken from the lower third of the screed thickness, away from the heating coils.

In summary, if the building schedule imposes reduced intervention times for finishing work and includes large open living spaces, anhydrite screed is the most rational technical choice. It eliminates the risk of shrinkage cracks and shortens the overall schedule thanks to the anticipated heating cycle. On the other hand, for any basement, garage, laundry room or wet room subject to running water, cement screed remains irreplaceable: it retains all of its compactness and mechanical strength, even if the tiling or waterproofing joint should fail during the lifespan of the structure.

Moisture damage and non-conformities: remedial protocols

The confrontation of a flowable or traditional mortar with an abnormal moisture source requires an immediate diagnosis of the binder. On a calcium sulphate screed, an accidental water inflow destroys the crystalline matrix if stagnation exceeds forty-eight hours. As soon as a flood or construction site leak is observed, technical drying using condensation dehumidifiers and sub-screed turbines must be deployed without delay. If the material becomes powdery on the surface under the tip of a scratch tool or loses its mechanical cohesion, complete removal of the saturated area is necessary down to the insulating blinding layer.

For cement screed, the main defects stem from poorly controlled differential shrinkage or too abrupt a heating-up. The appearance of random cracking or corner curling requires a topographical survey with a two-metre straightedge. Stabilised cracks without a level difference exceeding the tolerances of standard SIA 251 are subject to rigid bridging: opening the saw cut with an angle grinder, installing corrugated metal staples every twenty-five centimetres and injecting a quartz-filled epoxy resin to refusal.

  • Continuous infiltration on calcium sulphate: complete removal of the affected area, replacement of the wet insulation panel, followed by the pouring of a compatible mortar mechanically anchored to sound edges.
  • Persistent residual moisture on cement screed: strict prohibition on installing water vapour-tight parquet without prolonged resumption of the controlled heating cycle.
  • Non-adherent surface film: mechanical sanding with a diamond disc with integrated industrial vacuum extraction, followed by verification of surface hardness.

The joint inspection record logged on the construction site report protects the screed layer. Any decision regarding heavy resurfacing or partial demolition must receive formal approval from the site management prior to intervention.

Frequently asked questions

Must an anhydrite screed flooded by construction water damage be systematically demolished?

Not necessarily. If the stagnant water is pumped out within twenty-four to forty-eight hours and the underlying thermal insulation is not submerged, technical drying by air dehumidification can save the structure. On the other hand, if the mortar crumbles under the fingernail, has disintegrated into paste or if the underlying mineral wool remains saturated, the removal and complete repair of the affected span become inevitable according to trade rules.

Can large-format tiles be installed on a cement screed whose shrinkage is not complete?

This is a major risk of debonding or through-cracking. A cement screed undergoes hydraulic shrinkage for several months. If the basic drying time is not completed or if the residual moisture exceeds the limits prescribed by standard SIA 251, shear stresses exceed the adhesion of setting mortars. The creation of dividing joints and compliance with the waiting time remain essential.

How to react to a calcium sulphate screed that presents a powdery surface?

This surface film results from laitance rising due to excess mixing water or drying too early under a draft. The screed layer must perform mechanical sanding with a coarse-grain abrasive disc between seven and fourteen days after pouring. Complete dust extraction reveals the hard mineral skeleton essential for the mechanical bonding of adhesives and primers.

What to do when the residual moisture content blocks the installation of parquet on the eve of contractual deadlines?

No moisture-sensitive floor covering should be installed without compliance of the calcium carbide measurement. The construction manager must maintain controlled natural ventilation or set up mobile air dehumidifiers coupled with underfloor heating at a constant setting. The hasty application of a waterproof epoxy barrier is formally prohibited on anhydrite screed because it traps destructive moisture.

Texts and standards cited

  • SIA 251Floating screeds inside buildings, execution tolerances, shrinkage, drying and conditions of suitability for floor covering installation.

In the same section