Skip to content
Website
🧱 CFC 281Levelling compounds, industrial floors and screeder safetyChapter 1 of 10 in the section

Levelling compound: primer according to the substrate, permitted thickness and debonded levelling compound

This chapter details the preparation rules for successful floor levelling in accordance with the requirements of SIA 251. You will learn how to assess the absorption of the substrate screed, select the appropriate bonding primer, define application thickness limits, and prevent shear debonding caused by excessive differential shrinkage.

Key takeaways

  • The primer regulates substrate absorption to prevent the premature drying out of the levelling compound binder.
  • Application without a primer on a porous substrate causes matrix burning and dusting.
  • Each smoothing product specifies a minimum pouring thickness and a strict maximum limit.
  • Excessive thickness generates differential shrinkage that tears the levelling compound away from its substrate.

The bonding primer neutralises porosity and guarantees mortar setting.

A self-levelling smoothing mortar poured without a primer on a cement or calcium sulphate screed causes the system's adhesion to fail. The porous substrate absorbs the mixing water by capillarity with destructive rapidity. Deprived of its water of hydration, the cementitious binder undergoes brutal desiccation before its chemical set is complete. This phenomenon, known as burning, turns the base of the levelling compound into a powdery layer with no mechanical cohesion. SIA 251 states that mechanical preparation of the substrate, meticulous vacuuming and the application of a suitable primer are essential requirements before any smoothing work. A primer is never optional: it saturates surface porosity, neutralises capillary suction and enables the mortar to achieve all of its contractual mechanical strengths.

Burning of the smoothing mortar
Premature desiccation of the mineral binder caused by the instant suction of mixing water by an untreated porous substrate, blocking silicate hydration and destroying adhesion.

The mineral nature of the substrate determines the choice of primer. On an absorbent cement screed, the flooring contractor applies a synthetic dispersion diluted in accordance with the manufacturer's recommendations using a roller. This product penetrates the capillary network, binds the residual dust that escaped the vacuum and regulates the floor's absorbency. On a sanded calcium sulphate screed, a specific resin isolates the plaster from the cementitious components to prevent the formation of expansive ettringite. On a non-absorbent substrate such as degreased tiles or dense power-floated concrete, the role of the primer changes: it no longer slows down absorption, but provides essential anchoring roughness using calibrated silica grains.

Selection of the primer according to the porosity and mineral nature of the substrate
Screed substrateSubstrate absorptionType of primerTechnical role
Sanded cement screedOpen porosity and high suctionDiluted acrylic dispersionRegulates absorption and fixes dust
Calcium sulphate screedPorous and moisture-sensitiveEpoxy primer or dedicated barrierPrevents water attack and ettringite
Smooth concrete or tilesNone, dense and glazed surfaceQuartz-filled resinCreates mechanical bonding roughness
Surface-chalking screedHeterogeneous and insufficient cohesionFluid consolidation resinPenetrates to densify the surface zone

Observe the nominal thickness range to prevent shearing and debonding

Self-levelling smoothing mortars have a strict thickness range defined in the manufacturers' technical data sheets. In accordance with SIA 251, the minimum poured thickness must allow the product to flow freely under its own weight and form a continuous, dense and resistant layer. For a standard fluid compound, this lower limit is 2 millimetres to 3 millimetres. Applied below this technical threshold, the material does not spread well, hardens prematurely on contact with the ambient air and fails to compensate for substrate irregularities. The resulting layer remains fragile, erodes quickly under foot traffic and does not exhibit the indentation resistance required beneath the future floor covering.

Conversely, exceeding the maximum permitted thickness causes massive debonding through disc-like failure. The excessive increase in the volume of mortar increases the mass of mixing water, which considerably amplifies hydraulic shrinkage during setting. Since the product dries faster on the surface than at the core, severe differential shrinkage develops through the thickness. This phenomenon generates significant tensile stresses at the core of the mortar and severe shear forces at the bond line. As soon as these stresses exceed the surface cohesion of the screed or the adhesion of the primer, the levelling compound detaches abruptly, cracks in a network and sounds hollow when tested.

  1. Checking for unevennessIdentify irregularities using a 2-metre straightedge in accordance with SIA 251 to estimate the maximum thickness required.
  2. Selection of the mixChoose a fluid self-levelling compound up to 10 millimetres or a fibre-reinforced product suitable for make-up depths up to 30 millimetres.
  3. Setting out level markersGlue level markers at low points to control the pouring height and prevent accidental over-thicknesses.
  4. Levelling and de-aeratingGuide the material with a rake and then use a spike roller to drive out trapped air and neutralise surface tensions.

Porosity diagnosis and primer selection in accordance with SIA 251

On the construction site, acceptance of the substrate determines the final adhesion of the flooring system. Before spreading the smoothing mortar, the foreman or team leader assesses the porosity of the screed or slab in accordance with SIA 251. The water drop test is the most reliable direct diagnostic tool: a clean drop of water placed on a cleaned and vacuumed surface must disappear within one to three minutes. Instant absorption, under sixty seconds, reveals a hyper-absorbent substrate that will drain water from the mortar. Conversely, a bead of water lingering beyond five minutes indicates a glazed, sealed concrete or one polluted by curing agents.

Choice of primer according to the condition and absorption of the substrate
Substrate typeObserved porosityBonding primerTime before pouring
Porous cement screedAbsorption under 60 sDiluted synthetic dispersion2 to 4 hours
Calcium sulphate screedModerate absorptionEpoxy primer sanded to excess12 to 24 hours
Smooth concrete without porosityNo absorptionResin primer with silica3 to 6 hours
Stubborn adhesive residuesVariable and sealedEpoxy bonding bridge12 to 24 hours

On calcium sulphate screeds, the risk of chemical incompatibility strictly dictates the interface system. Direct contact between a mixed-binder levelling compound and plaster or anhydrite causes the crystallization of secondary ettringite in the presence of residual moisture. This highly expansive mineral decouples the levelling layer through irreversible molecular shear. The application of a reactive resin blocks all water transfer and provides a protective chemical barrier. On absorbent cementitious mineral substrates, the impregnation primer fulfills a purely physical function: it seals open pores, prevents bubbling caused by the outgassing of air trapped in the screed and neutralises the capillary suction effect that destabilises the hydraulic set of fast-setting self-levelling mortars.

Interface pathologies: desiccation by suction and shear in over-thickness

The phenomenon of burning threatens any levelling compound applied to a neglected or insufficiently impregnated absorbent substrate. As soon as the fluid paste is poured, the underlying porosity sucks out the mixing water via violent capillary action before the cement hydration reactions start. The mortar undergoes premature desiccation: on the surface, the skin appears hardened by the air set, but the internal matrix remains friable, porous and lacking mechanical consistency. This dehydrated compound exhibits no resistance to perpendicular tension. As soon as the final floor covering is subjected to dynamic loads or the finishing adhesive polymerises while developing its normal shrinkage tension, the levelling compound fails by internal delamination, leaving a thin powdery layer stuck to the back of the torn-off covering.

Debonding also results from exceeding the maximum thickness prescribed by the manufacturer and SIA 251 guidelines. All self-levelling mortars undergo hydraulic shrinkage during initial hardening. If the thickness exceeds the nominal level without the addition of a calibrated quartz filler (generally 0.4 mm to 0.8 mm particle size sand dosed according to the technical data sheet), volumetric shrinkage increases exponentially. The evaporation kinetics create a moisture gradient between the free surface and the base of the levelling compound, inducing differential tensile stresses. The material tends to curve upwards, initiating warping at the edges and corners. These tangential stresses quickly exceed the bond strength of the primer, causing erratic cracking followed by massive debonding in hollow-sounding plates under foot traffic.

To make good a subfloor where hollows exceed ten millimetres, the flooring contractor applies the material in successive passes after complete drying and re-application of a suitable primer, or resorts to a patching mortar with a firm consistency. Strict compliance with expansion joints and control joints in the underlying screed remains essential: no levelling compound, regardless of any reinforcement, can bridge an active movement joint without shearing.

Remediation protocol after delamination or premature desiccation

When the levelling compound sounds hollow, powders underfoot or blisters due to excessive differential shrinkage, this failure requires immediate methodical intervention. A self-levelling smoothing mortar that has debonded in layers due to the absence of a bonding primer or sheared due to a flagrant violation of permitted thickness limits can never be consolidated by surface impregnation. The unbonded crust forms a failure interface that ruins the cohesion of the flooring system in accordance with the adhesion requirements set by SIA 251.

  1. Mechanical purging down to a stable substrateRemove the entire non-adherent levelling compound using a wide chisel, floor milling machine or diamond grinder with integrated dust extraction. The mechanical action must lay bare the original concrete or sound mineral screed, leaving no powdery residue or residual patches around the edges.
  2. Vacuuming and cohesion checkRun the heavy industrial vacuum cleaner over the entire room to extract fines trapped in the microporosity. Test the compactness of the substrate by cross-scratching with a steel chisel or by a direct pull-off test to ensure that the substrate has the strength required by SIA 251.
  3. Saturating application of the suitable primerDistribute the bonding primer chosen according to the nature of the substrate using a roller or brush. On an absorbent mineral substrate, apply a regulating acrylic dispersion in two crossed passes if necessary; on a smooth, closed substrate, apply a sanded bonding primer. Scrupulously observe the drying window before mixing.
  4. Reconstitution within tolerance limitsPour the smoothing mortar while scrupulously observing the manufacturer's technical data sheet. If the local level difference exceeds the maximum thickness permitted for the neat product, incorporate oven-dried quartz sand in approved proportions or carry out the work in multiple passes after re-priming.

Remediation concludes with a flatness check using a 2-metre straightedge and systematic acoustic sounding with a tradesman's hammer after 48 hours of setting. This rigorous protocol restores the mechanical performance prescribed by SIA 251 and provides a secure substrate for the subsequent flooring installer.

Frequently asked questions

Can a self-levelling compound be poured directly onto a bare cement screed without a primer?

No, applying a primer is mandatory on bare cement screed. Without a regulating barrier, the porous mineral substrate instantly absorbs the levelling compound's mixing water by capillarity. This suction phenomenon deprives the cement of the water essential for its hydration, causing the paste to burn, surface dusting, rising air bubbles and rapid delamination under traffic loads, in breach of standard trade practices.

What are the technical risks of exceeding the maximum thickness authorised by the manufacturer?

Exceeding the maximum thickness generates massive hydraulic shrinkage during the curing of the mass. Shrinkage stresses create intense shear at the interface between the levelling compound and the substrate. The levelling layer then curls at its edges, cracks in a crazing pattern and ends up tearing away from the mineral substrate, sometimes taking the surface crust of the screed with it. For heavy thicknesses, the addition of approved quartz is essential.

What is the waiting time to be observed between applying the primer and pouring the levelling compound?

The time depends on the chemical formulation of the primer and the climatic conditions in the room. An acrylic emulsion on an absorbent screed generally requires between one and four hours of drying: the film must be dry to the touch without sticking to the shoe. Conversely, a sanded epoxy primer often requires a minimum curing period of twelve hours. Exceeding the maximum permitted time makes it necessary to reapply a layer to prevent loss of adhesion.

How do you identify whether an old substrate is too absorbent or sealed before choosing your primer?

The water drop test is carried out on the cleaned and vacuumed substrate. A few drops of clean water are placed in several representative locations. If the water is absorbed in less than a minute, the subfloor is excessively porous and requires an absorption-regulating diluted primer. If the water beads for more than five minutes without penetrating, the substrate is closed or glazed: it therefore requires mechanical abrading followed by a silica-filled bonding primer.

Texts and standards cited

  • SIA 251Floating and bonded screeds in construction, adhesion requirements and execution rules

In the same section