The hollow sound: local detachment, systematic sounding and repair by injection

A hollow sound on a bonded screed indicates a loss of bond with the concrete substrate. This chapter shows you how to identify these early-stage detachments during the acceptance inspection, map the voids accurately, and choose between repair via low-pressure injection of fluid epoxy resin or local demolition prior to tile installation.

Key takeaways

  • Systematic sounding with a screed maker's hammer reveals adhesion defects that are invisible to the naked eye.
  • Standard SIA 251 prescribes perfect bond continuity to prevent breakage of the final floor covering.
  • Any area producing a hollow sound is precisely marked out to quantify the affected surface area.
  • Resin injection restores monolithicity without requiring heavy, destructive removal work on the construction site.

Detecting the loss of bond: striking protocol and topographical survey of voids

On a bonded screed, the lack of intimate cohesion with the concrete substrate constitutes a critical defect. A debonded layer flexes under service loads, leading to premature tile breakage and joint shearing. Before notifying suitability for smoothing compounds or tile installation, the installation team must systematically inspect the entire hardened surface. This inspection allows for no visual approximation: a perfectly flat and trowelled mortar can conceal a complete detachment pocket caused by too rapid drying of the bonding slurry or residual dust that was not vacuumed during preparation.

Hollow sound in bonded screed
Clear and high-pitched acoustic resonance produced by mechanical impact on a screed, indicating an air gap or microscopic bond failure between the interposition mortar and the load-bearing slab.
  1. Systematic hammer inspectionThe applicator sweeps across the screed by tapping the floor with regular, small blows spaced 20 centimetres apart using a tiler's hammer or a 200-gram fitter's hammer. A solid, dull sound confirms the transmission of the wave into the slab; a sharper, vibrating resonance immediately reveals the underlying air void.
  2. Perimeter delineationAs soon as a clear sound is perceived, the taps are tightened in a star pattern every 5 centimetres to precisely locate the boundary where the sound becomes solid again. The bond failure line is drawn directly on the floor using an indelible grease chalk or construction marker.
  3. Survey on setting-out planEach identified zone is dimensioned relative to the structural axes and transferred to the layout plan of the work. This mapping makes it possible to calculate the ratio of detached surface area to the room and to identify whether the detachment runs along a joint, an internal corner or a concreting joint.

Remedial work: technical trade-off between epoxy injection and local chiselling

Faced with a mapped detached zone, the team leader decides between two intervention methods: repair by injection of a very fluid synthetic resin or the pure and simple removal of the hollow mortar. This choice depends directly on the surface area concerned, the thickness of the screed and the geometry of the air pocket. When the screed retains its surface mechanical integrity and shows no destructive map cracking, consolidation by injection avoids the harmful vibrations of chiselling and ensures compliance with the work schedule of other trades.

Decision criteria for treating local detachments
Observed configurationStructural diagnosisRecommended methodWorkshop precautions
Isolated pocket under 0.5 square metres without crackingInterface detachment due to local drying of the bonding bridgeInjection of liquid epoxy resin under low pressureCheck for absence of seepage through neighbouring joints
Hollow-sounding slab with microcracks and spallingDisintegrated mortar or locally insufficient thicknessClean cut with angle grinder, removal and hacking outReconstitution with shrinkage-compensated repair mortar
Linear detachment along a crack-control jointEdge lifting due to differential shrinkage or thermal stressWidening saw cut, dowel interlocking and injectionRespect for the exact location of the crack-control line
  1. Drilling injection pointsWithin the delineated zone, drill vertical holes with a diameter of 8 to 10 millimetres spaced 20 to 30 centimetres apart until reaching the interface with the load-bearing concrete. Meticulously vacuum drilling dust using an industrial vacuum cleaner equipped with a narrow nozzle to clear the circulation channels.
  2. Installation of injectors and sealingInstall metal packers or surface-glued plastic nozzles. If peripheral cracks are exposed, seal them with thixotropic epoxy mastic so that the injection binder does not escape freely without filling the void beneath the screed.
  3. Pouring and grouting with resinIntroduce a two-component epoxy resin of very low viscosity, either by gravity using vertical reservoirs or using a manual pump under low continuous pressure. Continue grouting until the resin rises into the adjacent vents, confirming the filling of the underside.
  4. Final inspection after curingAfter complete hardening according to the manufacturer's technical datasheet, grind the injectors flush with the floor. Perform a second systematic hammer inspection: the sound must have returned to a perfectly dull and homogeneous state across the entire formerly mapped pocket.

Execution of low-pressure epoxy injection

Resin injection under a debonded bonded screed restores monolithic continuity with the concrete slab without heavy demolition. This method applies when the hollow-sounding zone is stable under load, non-pulverulent and bordered by a perfectly bonded screed. A two-component epoxy resin of very low viscosity penetrates by capillarity and gravity into the interface void, filling detachments ranging from a few tenths of a millimetre to several millimetres.

  1. Drilling injection and degassing channelsDrill 6 to 10 mm diameter holes at the intersections of the mapped grid, spaced 20 to 30 cm apart. The drill bit must pass through the entire thickness of the screed and penetrate 5 to 10 mm into the load-bearing concrete. Drill peripheral vents at the edge of the detachment to guarantee the complete evacuation of compressed air.
  2. Dust removal and industrial vacuumingVacuum each hole with a tight reducing nozzle coupled to an industrial vacuum cleaner equipped with suitable filters. Briefly blow dry, oil-free compressed air into the boreholes to expel drilling flour trapped in the cleavage plane, then vacuum again to prevent internal clogging.
  3. Installation of injectors and sealing groutInsert suitable conical cannulas or injectors. If cracks are exposed on the surface of the screed, seal their path with thixotropic epoxy mastic or rapid-setting mortar to prevent the egress of liquid resin under the effect of pressure.
  4. Progressive resin injectionInject the fluid resin using a manual or pneumatic low-pressure pump, starting from the lowest or most central point towards the periphery. Continue pumping until a clear and continuous reflux of resin without bubbles appears through the neighbouring vents, then immediately seal the saturated injectors.

Local removal, reconstruction and final inspection according to standard SIA 251

When mapping reveals crushing of the underside, insufficient mortar thickness or a detached surface area exceeding injectability thresholds, repair requires targeted mechanical removal. The screed layer delineates the perimeter with a diamond disc cutter at a controlled depth to protect any reinforcement and avoid any initiation of uncontrolled cracking in the underlying concrete.

Technical comparison of repair methods for a detached bonded screed
Site criterionEpoxy resin injectionLocal removal and heavy smoothing compound
Interface void thicknessLess than 3 mm, clean cleavage planeGreater than 3 mm or presence of friable dust
Impact on scheduleCures in 24 hours, rapid tilingComplete drying of repair mortar required
Specific equipmentLow-pressure pump, cannulas, fluid resinFloor saw, light breaker, vacuum cleaner
Concrete substrate preparationNone (blind underside intervention)Shotblasting or bush hammering, sand-blasted epoxy bonding bridge
Residual riskInjection refusal if clogging dust is presentVisible construction joint to be mirrored if differential

After removing rubble and thoroughly cleaning the concrete substrate, reconstruction requires a resin mortar or a shrinkage-compensated mineral mortar mixed onto a fresh-on-fresh bonding bridge. The mortar must have an elastic modulus and compressive strength compatible with the existing work to avoid shear stresses at the connection.

Delivering a floor with untreated hollow areas transfers responsibility for defects onto the screed layer: under thermal and mechanical loads, the bonded covering will inevitably undergo shearing resulting in joint failure and tile debonding. The joint inspection report rules out any subsequent disputes between trades.

Dispute management and repair failure: widespread detachment and liabilities

When systematic hammer sounding reveals diffuse detachments over a large part of the room or if resin injection fails to restore cohesion, the screed layer faces a major risk of dispute with the tiler. A bonded screed that sounds hollow undergoes bending under service loads, breaking the tile adhesive shortly. If the resin reflux is nil or if the crack spits out unbonded pulverulent laitance, the mechanical adhesion with the underlying concrete slab is definitively compromised, precluding any floor covering installation.

Faced with detachment exceeding permitted tolerances or covering continuous surfaces too vast to be treated locally, overall removal of the bay is mandatory. The site manager must formalise a joint inspection record in writing without delay, in the presence of site management and the tiler. According to standard SIA 251, acceptance of the substrate by the floor covering installer seals the transfer of responsibility. Attempting to mask debonding with a surface smoothing compound fully engages the liability of the screed company when defects subsequently appear.

Decision tree upon finding repair failure
Acoustic and visual findingProbable technical causeSite decision
Persistent hollow sound after injectionIncomplete reflux or resin blocked by dustChiselling of the area and making a patch
Detachment greater than 20% of the bayFailure of the adhesion barrier or thermal shrinkageComplete removal of the bay and substrate repair
Through-crack along the repair jointPoor bridging or repair without fresh resinClean cut of the joint and dowel pinning

In the event of complete demolition prescribed by site management, mechanical scabbling of the load-bearing slab must eliminate all old mortar residue to restore the initial roughness of the concrete. Rubble and mineral waste are sorted and then disposed of in accordance with waste regulations. A new bonding bridge is mixed only on a perfectly clean, dust-free substrate saturated with water, guaranteeing the definitive absence of underlying voids when pouring the new screed.

Frequently asked questions

How to prove to the client that an injected area has been remediated?

Inspection is carried out via a new systematic hammer sounding after complete polymerisation of the resin, in the presence of site management. The acoustic change is immediate: the hollow sound gives way to a dry and solid ring. To remove any doubt on a sensitive surface, a 50-millimetre diameter control core drill allows visual verification of the filling of the cleavage plane and anchorage in the load-bearing concrete.

Can the tiler refuse to work on a screed repaired by injection?

The tiler examines the substrate prior to installation in accordance with professional rules. If hammer sounding confirms that the hollow sound has disappeared and flatness remains compliant with standard SIA 251, the substrate is considered acceptable. On the other hand, if residual pockets remain or if resin burrs hinder adhesive bonding, the CFC 282 craftsman records justified reservations and suspends installation until sanding or repair is completed.

Why does detachment often occur at edges or near sawn joints?

Hydraulic shrinkage stresses accumulate preferentially at slab ends and along cuts. If the bonding bridge dried before the mortar was spread or if wet curing was insufficient, tensile stresses exceed the pull-off strength of the interface. The edges lift imperceptibly through a warping effect, creating a detachment plane that sounds hollow during hammer sounding before any floor loading.

What is a frequent error when making a patch?

The classic error consists of making a connection without a clean cut using an angle grinder. A bevelled cut or feathered edges end up fraying and sounding hollow under construction traffic. The area must be delineated by a vertical saw cut at least fifteen millimetres deep, cleaned by industrial vacuuming, coated with a fresh epoxy bonding barrier, and then compacted vigorously with a shrinkage-compensated mortar compatible with standard SIA 251.

Texts and standards cited

  • SIA 251Execution specifications, tolerances and inspection of screeds in construction
  • ordonnance sur les déchetsSorting and recovery of mineral waste from deconstruction on site

In the same section