Key takeaways
- The surface laitance of a calcium sulphate screed prevents any adhesion of the subsequent bonded floor covering.
- Mechanical laitance removal sanding is an integral part of the standard service provided by the CFC 281 screed layer.
- Direct industrial vacuum extraction captures fine dust as the single-disc machine with abrasive grit passes over the floor.
- SIA 251 governs surface acceptance prior to the installation of adhesives and self-levelling compounds.
Surface laitance on anhydrite screed and adhesion criteria
During the pouring of a calcium sulphate-based fluid screed, the finest components, binder residues, and excess water rise by sedimentation. In the open air, this phenomenon creates a whitish, fragile, and friable surface film, commonly known as anhydrite surface laitance. This skin has virtually zero mechanical cohesion. If an applicator attempts to bond a floor covering directly or apply a primer without mechanical preparation, failure will not occur within the adhesive, but within this film which has delaminated from the screed body.
- Anhydrite laitance
- Powdery, non-adherent surface layer formed by bleeding and the migration of fine binder particles to the top of the fluid screed during its initial setting phase.
SIA 251 sets out quality requirements for screeds and mandates a substrate with a stable, flat, clean, and mechanically resistant surface. On traditional cement screeds, the surface finish is generally achieved during installation by manual or mechanical smoothing using a power trowel, often called a helicopter. This smoothing tightens the grain and makes the surface compaction uniform. Conversely, for a calcium sulphate self-levelling screed, smoothing is impossible during the setting process. Achieving a compliant surface strictly requires subsequent treatment by mechanical abrasion.
The stripped surface must present a rough condition revealing the granular skeleton of the matrix. The adhesion of the bonded covering depends entirely on the tensile strength of this contact zone. For a tiler or parquet installer, the cross-cut test or scratching with a screwdriver must reveal sound material, free from powdery dust, guaranteeing the mechanical grip of adhesive mortars or modern bonding systems.
The sanding and vacuuming process according to trade rules
The mechanical laitance removal of a fluid screed is an integral part of the screed layer's service and must be included in the finishing operations specified in the construction contract. This operation is generally carried out between the fourth and tenth day after pouring, as soon as the screed can be walked on and its initial hardening allows machines to pass without damaging the edges. Waiting several weeks before treating the laitance increases the hardness of the crust, complicates the operation, and prematurely wears out abrasive tooling.
- Surface hardness checkVerify that the screed resists the imprint of a work boot and that the surface no longer marks under a moderate concentrated load.
- Single-disc mechanical sandingPass a heavy single-disc machine or floor sander equipped with a 16 or 24 grit silicon carbide disc, or diamond segments suitable for plaster screeds.
- Exposing the aggregatesContinue the cross-passes until the dull white film is completely removed and the hard granular mix clearly appears.
- Immediate industrial vacuumingConnect a professional vacuum cleaner of the appropriate class directly to the sander's shroud, then complete with a thorough vacuum sweep of the room.
| Characteristic | Traditional cement screed | Calcium sulphate fluid screed |
|---|---|---|
| Finishing method | Manual smoothing or power trowel in plastic phase | Mechanical sanding after partial hardening |
| Timing of treatment | A few hours after screeding to the guide rails | Between 4 and 10 days after pouring |
| Surface behaviour | Limited bleeding film if properly smoothed | Continuous and friable calcareous and sulphatic laitance |
| Requirement for stripping | Depending on surface condition and planned covering | Mandatory for any bonded system |
| Typical equipment | Power trowel or rotary smoothing machine | Abrasive single-disc machine with industrial vacuum system |
The evacuation of the generated dust constitutes a critical phase. Simple manual sweeping disperses volatile elements into the air and redeposits a film of dust that clogs the open pores of the substrate. Connecting a sealed industrial vacuum unit to the machine shroud allows dry working while complying with the Ordinance on Construction Work regarding air quality in the workplace. The final surface must be free from powdery residues before being jointly accepted.
Execution distinction: cement smoothing and anhydrite sanding
Surface treatment fundamentally depends on the mineralogical composition of the binder used. On a traditional cement screed, surfacing is carried out during the setting phase using a rotary power trowel (helicopter) or by careful manual smoothing using a plastic or magnesium float. This mechanical action aims to compact the fresh mortar, tighten the surface grain, and comply with the flatness tolerances prescribed by SIA 251. Conversely, the calcium sulphate-based fluid screed is never smoothed. Its self-levelling consistency precludes the use of rotary machines in the fresh phase: the finish is achieved solely through a cross-pass of the levelling bar during pouring to remove bubbles from the mass and set levels.
On a cement mortar, the main risk lies in premature or prolonged surfacing. Persistent mechanical action on bleeding mortar brings up mixing water laden with fine particles and cement hydrates. This forms a fragile surface film likely to powder under the traction of adhesives. On anhydrite, the laitance does not result from an execution error, but from a normal sedimentation reaction: excess water rises to the surface dragging residual sulphates and additives. This vitrified or chalky crust blocks carbonation and slows down the evaporation of water. Sanding is not a spot retouch, but a mandatory substrate-opening operation integrated into the screed layer's service.
| Execution criterion | Cement-based screed (CT) | Calcium sulphate screed (CA) |
|---|---|---|
| Surfacing method | Manual smoothing or mechanical finishing with a rotary trowel | Cross de-aeration with a levelling bar without smoothing |
| Timing of action | During setting, as soon as the mortar can support a worker | After partial hardening of the matrix (3 to 14 days) |
| Finishing tool | Petrol or electric rotary power trowel blades | Single-disc machine or heavy floor sander with abrasive discs |
| Surface film | Possible laitance in case of excessive bleeding | Systematic laitance due to binder sedimentation |
| Risk without treatment | Mortar powdering and low pull-off strength | Watertight film preventing drying and bonding |
Substrate acceptance, dust removal, and preparation for bonded installation
According to the requirements defined by SIA 251, a floating screed must provide a flat, clean, and mechanically cohesive surface to receive durable bonded coverings. If the calcium sulphate-based screed is not properly sanded, its surface film exhibits negligible tensile strength. During the setting of a tile adhesive or under the effect of solid parquet shrinkage, the shear stresses exceed the low cohesion of this crust. Failure does not occur in the adhesive joint, but tears off the friable surface layer of the screed body, leading to complete and irreversible delamination of the work.
Industrial vacuuming is the inseparable extension of mechanical treatment. Anhydrite sanding releases very fine dust that immediately clogs the open pores of the hardened mortar. The use of an industrial construction vacuum cleaner for fine dust with enhanced filtration is mandatory to clean the installation base. Ordinary sweeping is strictly prohibited: it merely moves the residues and fills the micro-asperities necessary for adhesion. Without deep extraction, the adhesion primer essential before bonding will not penetrate the crystal network of the screed and will form a floating film destined to delaminate.
The control of mechanical strength is carried out through direct checks on the work before any installation authorization. The sclerometer scratch test or knife cross-cut test is used to evaluate surface hardness: the drawn grooves must remain sharp, without crumbling or material tearing at the intersections. In case of doubt or for floor coverings subjected to heavy loads, a pull-off adhesion test on a glued metal disc measures the effective breaking value. If cohesion is insufficient or if a chalky film remains, an additional sanding pass with diamond segments is necessary to expose the sound matrix.
Disputes and remedial work: curative treatment of hardened laitance
When the sanding of a calcium sulphate fluid screed has been omitted or carried out too late, the surface film dries and forms a compact vitrified crust. Appearing solid, this crust has no mechanical cohesion with the screed body. The tiler or parquet installer, required to check the substrate before their work, will refuse surface acceptance if they notice powdering during the scratch test or delamination during adhesion tests.
- Surface cohesion diagnosisCheck the depth of the degraded zone by cross-scratching. If the laitance forms a thick crust, measure the surface hardness to determine the exact thickness of material to be removed before reaching sound mortar.
- Milling or aggressive diamond sandingReplace paper discs with metal-bonded diamond segments. Work in regular cross-passes with a heavy floor sander, with simultaneous slaved vacuum extraction, until the aggregates reappear.
- Complete vacuuming and joint inspectionRemove all fine dust using an industrial vacuum cleaner equipped with suitable filters. Organize a joint visit with the installer of the final covering to formally record the compliance of the exposed substrate.
SIA 251 specifies that the screed must be delivered free of non-adherent particles, dust, and laitance. If the screed applicator attempts to pass this burden onto the covering installer, the client may demand remedial work at the screed company's expense. According to standard construction contract rules governed by the Code of Obligations and SIA 118, the removal of the surface skin is an integral part of the screed layer's service. In the event of corrective intervention, excess gypsum dust requires rigorous extraction to guarantee operator health in accordance with the requirements of the Ordinance on Construction Work.
Frequently asked questions
Who must pay for sanding if the tender does not explicitly mention this line item?
According to SIA 251, the removal of surface laitance on an anhydrite screed is an integral part of the screed layer's services. Even if the descriptive quote does not contain a separate item for this task, the delivered work must be ready to receive the adhesion primer. The contractor cannot claim a supplement for an operation essential to the technical compliance of their screed, unless expressly stipulated otherwise in the construction contract.
Can tiling be installed directly on anhydrite laitance without prior sanding?
This is strictly prohibited. The laitance consists of residual binder, bled water, and micro-dust with no pull-off strength. If tile adhesive is applied to this powdery layer, mechanical adhesion is zero. As soon as the heating is turned on or under thermal expansion stresses, the adhesive detaches along with the calcium sulphate surface film. The tiles quickly sound hollow, then lift off across entire areas of the floor.
What maximum time limit must be observed before sanding a calcium sulphate liquid screed?
Sanding is ideally carried out between seven and fourteen days after pouring, as soon as the screed is walkable and sufficiently hard at the surface. If one waits beyond three to four weeks, the laitance dries, crystallizes, and hardens considerably. The work then requires much more expensive diamond metal abrasives instead of simple silicon carbide discs. Early sanding also accelerates the core drying of the mortar.
Why is manual sweeping prohibited after sanding an anhydrite screed?
Sweeping merely moves the dust without removing the ultrafine particles embedded in the open pores of the mortar. These powdery residues form a separating film that prevents the penetration of the bonding resin or adhesive. Only an industrial vacuum cleaner with a fine dust filter guarantees the opening of capillaries. In addition, the Ordinance on Construction Work mandates limiting the dispersion of mineral dust in the air breathed on the construction site.
Texts and standards cited
- SIA 251Screeds in construction: execution specifications, surface conditions, and laitance removal
- SIA 118General conditions for the execution of construction work: delivery rules and defect rectification