Skip to content
Website
🧱 CFC 281Drying, heat-up and moisture measurementsChapter 8 of 10 in the section

Depending on the flooring: tiles, parquet, resin, and three different thresholds

A screed is not declared ready in absolute terms: its dryness state depends exclusively on the flooring that will cover it. This chapter allows you to precisely determine the required residual moisture threshold according to SIA 251, identify damage risks specific to parquet, tiles and resin, and properly record the calcium carbide test results.

Key takeaways

  • The residual moisture tolerance varies from single to triple depending on the watertightness of the applied flooring.
  • A bonded parquet requires a dried substrate to prevent cupping and shearing of the adhesives.
  • Synthetic resins block any vapor migration and require strict dryness to prevent blistering.
  • The calcium carbide test according to SIA 251 is the only valid reference before installation.

The permeability of the upper assembly dictates the required drying level

On Swiss construction sites, the classic mistake is to set an installation date based on the pouring schedule or a theoretical curing period. However, the evaporation rate of a screed depends on its thickness, building temperature, ambient ventilation, and whether or not underfloor heating is embedded. Above all, the target residual moisture value is not a constant inherent to the mortar: it is dictated by the water sensitivity and vapor permeability of the material covering the floor assembly.

Vapor permeability of the flooring
Ability of a floor assembly to allow residual gaseous moisture from the screed to pass through to the ambient air without mechanical, chemical or dimensional degradation of its components.

Laying ceramic tiles tolerates a higher amount of free water because cement grout joints allow gradual and slow evacuation of water vapor into the room. Conversely, wood parquet is a living hygroscopic material. If bonded to a substrate that is too wet, it absorbs the excess water through its underside, leading to differential swelling, cupping of the boards and, in extreme cases, lifting of the screed or delamination of the adhesive bed through shearing.

The binder type also alters the behavior of the screed. A cement-based screed undergoes slow chemical hydration which consumes a fraction of its residual water, but retains active capillarity. A fluid or troweled calcium sulfate screed loses all mechanical strength and degrades irreversibly if saturated with water trapped under an impermeable film. This is why standard SIA 251 modulates requirements based on these two combined parameters: the binder used and the nature of the flooring specified in the execution plans.

Limit thresholds according to standard SIA 251 and the CM testing procedure

Suitability to receive the flooring must be checked before installation work begins. The moisture content is determined using a calcium carbide device (CM device) on a sample taken across the entire thickness of the screed.

Norme SIA 251
Maximum admissible residual moisture contents for installation according to standard SIA 251 (CM values in percentage by mass)
Type of planned flooringCement screed without heatingCement screed with underfloor heatingCalcium sulfate screed without heatingCalcium sulfate screed with underfloor heating
Ceramic or natural stone flooring (adhesive mortar installation)2.5 % CM1.5 % CM0.5 % CM0.3 % CM
Bonded parquet (solid or multilayer wood)2.0 % CM1.5 % CM0.5 % CM0.3 % CM
Watertight resin flooring or watertight textile flooring2.0 % CM1.5 % CM0.5 % CM0.3 % CM

For the screed layer, responsibility ends with the delivery of a screed conforming to its strength class, correctly heated up according to the established thermal protocol, and accepted with an official moisture report. The 1.5 % CM threshold for bonded parquet on heated cement screed represents a strict requirement. This value generally cannot be achieved without complete and methodical heat-up of the underfloor heating system, conducted under the responsibility of the heating installer and documented day by day.

Sampling for the CM flask must obligatorily be carried out in the lower third of the screed thickness, where moisture is most concentrated, while carefully avoiding piercing the heating pipes concealed within the mass. The screed layer marks witness areas during execution to allow this secure core sampling.

Residual moisture thresholds depending on the finishing flooring

The screed layer delivers work whose free water content must strictly correspond to the nature of the flooring specified in the execution plans. While the tile setter can accommodate a substrate with moderate residual moisture thanks to permeable mineral grout joints, the parquet layer and synthetic resin applicator require a significantly drier substrate. Standard SIA 251 sets reference limit values to be measured using the calcium carbide method (CM bomb). These values do not depend solely on the composition of the screed binder — Portland cement or calcium sulfate —, but are directly dictated by the water vapor permeability of the final flooring and by the presence or absence of underfloor heating.

Residual moisture limit values according to standard SIA 251 (CM measurement)
Type of screedCeramics and natural stoneBonded parquetWatertight synthetic resin
Cement screed without heating≤ 2.3 % CM≤ 2.0 % CM≤ 2.0 % CM
Heated cement screed≤ 1.8 % CM≤ 1.5 % CM≤ 1.5 % CM
Calcium sulfate screed without heating≤ 0.5 % CM≤ 0.5 % CM≤ 0.5 % CM
Heated calcium sulfate screed≤ 0.5 % CM≤ 0.3 % CM≤ 0.3 % CM

Reading these values highlights a major technical requirement. On a heated cement screed, the difference between tiles (1.8 % CM) and bonded parquet (1.5 % CM) seems minimal on paper, but it often represents two to three weeks of additional drying time on the construction site or a prolonged temperature increase cycle. For calcium sulfate screeds, the material exhibits extreme sensitivity to residual water: moving from 0.5 % to 0.3 % CM ensures almost complete evacuation of free interstitial water, which is essential to prevent any subsequent degradation under a fully watertight assembly.

Degradation mechanisms of parquet and resins under the effect of residual water

Wood is a living hygroscopic material that constantly seeks moisture equilibrium with its substrate. When solid or engineered parquet is bonded to a screed whose moisture level exceeds the prescribed thresholds, the trapped water cannot escape upwards due to the varnished or oiled finish. It is absorbed by the underside of the boards, causing a moisture differential across the thickness of the wood. This imbalance generates massive tangential stresses: cupping of the boards, deformation of the edges, surface cracking and shear failure of the adhesive bed or screed surface. Conversely, ceramic tiles are inherently resistant to moisture; excess water evacuates slowly through the joint mortar without creating destructive pressure on the installation interface.

The application of an epoxy or polyurethane resin poses an even more radical physical constraint. The polymerized film forms a barrier completely impermeable to gases and liquid water. If the underlying screed contains a residual amount of water exceeding the admissible threshold, the heat-up or thermal fluctuations lead to evaporation under tension. Finding no outlet, this vapor pressure causes debonding through osmotic blistering and mechanical delamination of the flooring. On a calcium sulfate screed trapped under a watertight synthetic film, persistent residual moisture combined with heat gradually dissolves the crystal lattice of the gypsum, reducing the surface layer to non-cohesive dust.

This control chain implies flawless coordination during site management. If site management decides during the project to replace tiles with parquet on a heated cement screed, the installation deadline cannot be kept identical. Lowering residual moisture from 1.8 % to 1.5 % CM requires adjusting the general schedule, maintaining ventilation systems and prohibiting any temporary watertight covering on the screed. Neglecting this adjustment inevitably leads to a refusal of the substrate by the parquet layer during contradictory acceptance, or to a major dispute resulting from wood deformations.

Corrective measures in case of moisture threshold exceedances

When the calcium carbide device indicates a residual moisture level higher than the limits set by standard SIA 251, installation is strictly prohibited. While a value of 2.0 % CM on a cement screed allows the installation of ceramic tiles, it formally prohibits that of bonded parquet or watertight resin. Faced with a blocked schedule, the screed layer and site management must implement proportionate technical solutions without prematurely engaging the liability of the finishing contractors.

  1. Thermal reheating and technical dryingIf the underfloor heating is operational, a controlled heating cycle is restarted in coordination with the heating installer, without exceeding the authorized flow temperatures. In the absence of underfloor heating or for a calcium sulfate screed, condensation or adsorption dehumidifiers are installed, combined with air circulators. Air flows must sweep the surface homogeneously to prevent any shrinkage differential.
  2. Application of a vapor barrier or epoxy barrierWhen deadlines prevent waiting for natural evaporation for bonded parquet, the application of a two-component epoxy primer acting as a barrier against residual moisture constitutes a recognized technical option. This option requires the written agreement of site management and the parquet layer, and only applies to cement screed exhibiting sufficient surface cohesion, never to damp calcium sulfate.
  3. Contradictory check and reportAny new CM measurement must involve deep sampling in the thickest or least ventilated areas. The results are recorded in a contradictory protocol signed on site by the screed layer and the installer of the relevant flooring, formally recording whether or not the specific threshold has been reached.

Frequently asked questions

Why does parquet require a drier substrate than stoneware tiles?

Wood is a living hygroscopic material. Residual moisture exceeding 1.5 % CM on a heated cement screed causes upward water migration toward the wood. The boards swell, deform through cupping and shear the adhesive. Tiles, being an inert mineral material combined with vapor-permeable adhesives and cement grouts, tolerate higher water residue without the risk of immediate debonding.

Can a watertight resin be laid on a cement screed measured at 2.0 % CM?

No. Standard SIA 251 prescribes a strict threshold of less than or equal to 1.5 % CM for synthetic coatings poured without a draining underlay. An epoxy or polyurethane resin forms a film completely impermeable to vapor. The trapped water accumulates under the film due to thermal variations, creating osmotic pressures that cause blistering, generalized debonding and surface degradation.

Who is responsible for the moisture measurement authorizing the parquet layer to intervene?

Each trade must check the condition of the substrate before its work. The screed layer certifies the completion of the drying and heating protocol, but the parquet layer has the professional duty to carry out their own CM measurement before starting installation. If they note an exceedance of the permitted threshold for their type of installation, they must notify a notice of work interruption to site management.

How to treat a calcium sulfate screed that does not drop below 0.5 % CM?

To lay bonded parquet on a non-heated anhydrite screed, the mandatory threshold is 0.5 % CM. If the level stagnates, the absence of infiltrations must be checked, the surface film sanded to open the porosity, and professional dehumidifiers installed with sequential ventilation. Applying an epoxy barrier to block water is ruled out: calcium sulfate loses all strength if confined in a damp environment.

Texts and standards cited

  • SIA 251Floating and bonded screeds in buildings: requirements, execution and residual moisture checks

In the same section